Non-vulcanized Natural Rubber — Evolded Gas Analysis (TG-GC-MS)

TG-DTG-TIC plot of non-vulcanized Natural Rubber (NR), 3.36 mg, N2, continuous injection of the evolved gases at 1-min intervals.

A constant high temperature is maintained in the GC column to allow the gas mixture to pass quickly and separate into its main components. (measurement with TG-GC-MS).

At the onset of the NR Decomposition reactionA decomposition reaction is a thermally induced reaction of a chemical compound forming solid and/or gaseous products. decomposition (32 min., 346.3°C), the primary volatile products are isoprene C5H8 (peak 1 in TIC chromatogram) and 1-methyl-4-(1-methylethenyl)-cyclohexene C10H16 (peak 2).

This continuous GC-MS mode shows the gas evolution as a function of temperature and time and allows for the selection of individual mass numbers (m/z) for continuous plotting as a function of temperature (single ion monitoring, SIM).

The second stage of the NR Decomposition reactionA decomposition reaction is a thermally induced reaction of a chemical compound forming solid and/or gaseous products. decomposition (onset at 38 min., 406.2°C) is characterized by the evolution of products in addition to isoprene and substituted cyclohexene (as shown above). These can be identified as 5,5-dimethyl-1,3-cyclopentadiene (C7H10, 94 m/z), 1-methylene-2-vinylcyclopentane (C8H12, 108 m/z) and beta-humulene (C15H24, 204 m/z).

TG-DTG-TIC plot displaying thermal behavior of non-vulcanized natural rubber during gas analysis at varying temperatures.
TIC chromatogram showing gas evolution of non-vulcanized natural rubber, with peaks for isoprene (C5H8) and cyclohexene (C10H16) at specific temperatures.