Composition of a Bicycle Tire Casing

Introduction

Many people consider a bicycle to be an indispensable means of transportation. The tire is an elementary component and at the same time, a decisive influential factor on the riding characteristics. It can be adapted to suit the ground and desired riding quality qualities. 

Basically, a bicycle tire casing consists of a composite of different materials. This composite combines the flexibility and tribological properties of a rubber compound (tread) with the strength of a synthetic polymer fabric (carcass) and the dimensional stability of a wire bundle (core). The rubber compound itself is made of various organic and inorganic raw materials and fillers. This composition is largely responsible for the properties of the rubber compound. [1] 

Thermogravimetric analysis is a widely used analytical method for examining rubber compounds. Thermogravimetry is described in ISO 9924 and ASTM E1131 standards for this application range. Therefore, the composition of the casing of a bicycle tire is here examined using thermogravimetric analysis.

Methods and Sample Preparation

In order to obtain a measurement representative of the rubber compound of the casing, several small samples with a total mass of 10 mg were cut out of the casing profile. Care was taken to ensure that these pieces consisted only of the rubber compound of the tread and did not include any components of the carcass or the core. 

For the thermogravimetric investigation, the NETZSCH TG Libra® was employed. These measurements were carried out under the conditions detailed in table 1.

Table 1: Measurement conditions of the thermogravimetric investigation of a bicycle tire casing

SampleBicycle tire casing
Sample weight9.79 mg
Crucible materialAlumina, open
Temperature range40°C to 1100°C
Temperature program40°C - 850°C in nitrogen; 805°C - 1100°C in air
Heating rate10 K/min
AtmosphereNitrogen, air

Measurement Results and Discussion

Figure 1 shows the thermal Decomposition reactionA decomposition reaction is a thermally induced reaction of a chemical compound forming solid and/or gaseous products. decomposition of the bicycle tire casing. The first mass loss of 8.7% (DTG peak at 283.2°C) is due to the evaporation of the plasticizer content. Then, degradation of the organic rubber components can be observed. This takes place in two clearly separate steps with the first step showing a mass loss of 25.1% and the second one a mass loss of 31.8%. The two steps can also be recognized when looking at the DTG curve with the first peak at 379.1°C and the second peak at 469.8°C.

In addition to the organic components of the tire casing, small content levels of inorganic fillers can also be seen in the TGA curve upon further heating. This loss is due to the release of CO2 from the Decomposition reactionA decomposition reaction is a thermally induced reaction of a chemical compound forming solid and/or gaseous products. decomposition of CaCO3 into CaO at a peak of the DTG signal at 664.5°C. Even small amounts the 1.2% in this example can be detected without any problems. 

At 850°C, the atmosphere was switched from an inert nitrogen atmosphere to an oxidizing atmosphere. Due to this change of atmosphere, combustion of Carbon BlackTemperature and atmosphere (purge gas) affect the mass change results. By changing the atmosphere from, e.g., nitrogen to air during the TGA measurement, separation and quantification of additives, e.g., carbon black, and the bulk polymer can become possible.carbon black can be observed during heating to 1100°C, and the resulting Ash ContentThe ash is a measure of the mineral oxide content on a weight basis. Thermogravimetric analysis (TGA) in an oxidative atmosphere is a well-proven method to determine the inorganic residue, commonly referred to ash, in organic materials such as polymers, rubbers, etc. Therefore, the TGA measurement will identify if a material is filled and calculates the total filler content.ash content of 7.1% can be quantified.

Graph showing temperature-dependent mass changes of a bicycle tire casing with detailed curves for mass change rates and gas flow.
1) Temperature-dependent mass changes of a bicycle tire casing (green curve), rate of mass change (DTG, dashed blue curve), gas flow (nitrogen: dashed black; air: dashed blue).

Summary

The rubber compound of the bicycle tire casing was examined using thermogravimetric analysis. The proportion of organic ingredients, such as plasticizers and rubber, can thus be determined. Despite its low proportion, the inorganic filler content was additionally detected and the resulting Ash ContentThe ash is a measure of the mineral oxide content on a weight basis. Thermogravimetric analysis (TGA) in an oxidative atmosphere is a well-proven method to determine the inorganic residue, commonly referred to ash, in organic materials such as polymers, rubbers, etc. Therefore, the TGA measurement will identify if a material is filled and calculates the total filler content.ash content was determined.