SBR: Styrene-butadiene rubber

EM

Elastomers

General Properties

Short Name: SBR

Name: Styrene-butadiene rubber


Styrene butadiene rubber (SBR), manufactured from 1,3-butadiene and styrene, is the most widely used synthetic rubber. It usually contains 23.5% styrene and 76.5% butadiene. The rubber shows increasing thermoplastic properties with increasing styrene content, yet remains curable. With 1,3-butadiene as a co-monomer, cis-trans-isomerism also occurs.

Structural Formula

A minimalist black icon representing a light bulb surrounded by a circle, symbolizing innovation and ideas in analysis and testing.

Properties

Glass Transition TemperatureThe glass transition is one of the most important properties of amorphous and semi-crystalline materials, e.g., inorganic glasses, amorphous metals, polymers, pharmaceuticals and food ingredients, etc., and describes the temperature region where the mechanical properties of the materials change from hard and brittle to more soft, deformable or rubbery.Glass Transition Temperature-55 to -35°C
Melting Temperatures and EnthalpiesThe enthalpy of fusion of a substance, also known as latent heat, is a measure of the energy input, typically heat, which is necessary to convert a substance from solid to liquid state. The melting point of a substance is the temperature at which it changes state from solid (crystalline) to liquid (isotropic melt).Melting Temperature(-20)°C
Melting Temperatures and EnthalpiesThe enthalpy of fusion of a substance, also known as latent heat, is a measure of the energy input, typically heat, which is necessary to convert a substance from solid to liquid state. The melting point of a substance is the temperature at which it changes state from solid (crystalline) to liquid (isotropic melt).Melting Enthalpy(170 (cis)) J/g
Decomposition reactionA decomposition reaction is a thermally induced reaction of a chemical compound forming solid and/or gaseous products. Decomposition Temperature435 to 470°C
Young's Modulus2 to 10 MPa
Coefficient of Linear Thermal Expansion (CLTE/CTE)The coefficient of linear thermal expansion (CLTE) describes the length change of a material as a function of the temperature.Coefficient of Linear Thermal Expansion180*10-6/K
Specific Heat Capacity1.88 to 2.00 J/(g*K)
Thermal ConductivityThermal conductivity (λ with the unit W/(m•K)) describes the transport of energy – in the form of heat – through a body of mass as the result of a temperature gradient (see fig. 1). According to the second law of thermodynamics, heat always flows in the direction of the lower temperature.Thermal Conductivity0.20 to 0.25 W/(m*K)
DensityThe mass density is defined as the ratio between mass and volume. Density0.94 g/cm³
MorphologyRubber with hard and soft segments
General propertiesGood aging and abrasion resistance
ProcessingCross-linking by means of sulfur accelerating systems or peroxides
ApplicationsTire industry (cap of tires). Technical rubber goods (conveyor bands, seals). Mechanical engineering. Household articles (e.g., shoe soles)

NETZSCH Measurement

Differential Scanning Calorimetry (DSC) graph showing heat flow vs. temperature for two heating cycles, highlighting key transition temperatures.
Sample Mass13.10 mg
Heating Rates10 K/min
CrucibleAl, pierced lid
AtmosphereN2 (40 ml/min)

Evaluation

In the DSC curve from the1st heating (blue), SBR shows a Glass Transition TemperatureThe glass transition is one of the most important properties of amorphous and semi-crystalline materials, e.g., inorganic glasses, amorphous metals, polymers, pharmaceuticals and food ingredients, etc., and describes the temperature region where the mechanical properties of the materials change from hard and brittle to more soft, deformable or rubbery.glass transition at -45°C (midpoint), a broad, complex melting transi- tion (with peak temperatures at 19°C and 58°C and a melting enthalpy of approx. 6 J/g), caused by the melting of additives and an ExothermicA sample transition or a reaction is exothermic if heat is generated.exothermal effect (peak temperature: 168°C, enthalpy: approx. 10 J/g) that can be attributed to post-vulcanization. This ExothermicA sample transition or a reaction is exothermic if heat is generated.exothermal effect is absent in the2nd heating (red) after controlled cooling, indicating that vulcanization was completed in the1st heating. As a result, theTg in the2nd heating is shifted to a slightly higher temperature (midpoint of -44°C compared to -45°C in the1st heating). The step height (ΔSpecific Heat Capacity (cp)Heat capacity is a material-specific physical quantity, determined by the amount of heat supplied to specimen, divided by the resulting temperature increase. The specific heat capacity is related to a unit mass of the specimen.cp) of approx. 0.5 J/(g·K) remained almost unchanged. This small effect of post-cross-linking on temperature and height of the Glass Transition TemperatureThe glass transition is one of the most important properties of amorphous and semi-crystalline materials, e.g., inorganic glasses, amorphous metals, polymers, pharmaceuticals and food ingredients, etc., and describes the temperature region where the mechanical properties of the materials change from hard and brittle to more soft, deformable or rubbery.glass transition step is typical for elastomers. A melting transition due to additives with peak temperatures of 23°C and 34°C and an enthalpy of approx. 4 J/g is also seen in the DSC curve of the2nd heating.