Heat Flow Meter (HFM) with Instrumentation Kit: Measurements on Pyrex® – in Good Agreement with the Laser Flash Analysis (LFA) and Literature

Introduction

The Heat Flow Meter (HFM) technique is a well-known and accepted method to determine the Thermal ConductivityThermal conductivity (λ with the unit W/(m•K)) describes the transport of energy – in the form of heat – through a body of mass as the result of a temperature gradient (see fig. 1). According to the second law of thermodynamics, heat always flows in the direction of the lower temperature.thermal conductivity of insulating materials like EPS, rock-wool or glass-fiber boards. Also building materials like concrete with higher Thermal ConductivityThermal conductivity (λ with the unit W/(m•K)) describes the transport of energy – in the form of heat – through a body of mass as the result of a temperature gradient (see fig. 1). According to the second law of thermodynamics, heat always flows in the direction of the lower temperature.thermal conductivity and stiff structure can be investigated with the HFM. The Instrumentation Kit extends the measurement range up to 2 W/(m∙K). This application note describes the Instrumentation Kit in detail, and presents data obtained on Pyrex® with the HFM 436/3/1 (figure 1). Its effectiveness is demonstrated by correlating the data with the Laser Flash Analysis (LFA, figure 2) technique.

HFM 436/3/1 Lambda thermal analysis device by NETZSCH, designed for precise heat flow measurements in testing applications.
1) HFM 436/3/1 Lambda
LFA 467 HyperFlash thermal analyzer featuring a modern design and user-friendly interface for efficient thermal conductivity testing.
2) LFA 467 HyperFlash®

Instrumentation Kit

When testing insulating materials with the HFM technique, the interface thermal resistances between the specimen and the HFM plates are usually negligible, relative to the specimen´s thermal resistance. In case of high conductive and/or stiff samples, this assumption is no longer valid. Even if the specimen´s surfaces are very flat and planeparallel, there always remain some small air gaps at the interface, leading to significant differences between the plates´ and the specimen´s surface temperatures, and an inhomogeneous heat flow through the sample. To avoid these shortcomings, the Instrumentation Kit is necessary. It consists of two external thermocouples, and of two interface layers (figure 3). The interface layers improve the thermal contact between the plates and the specimen, while the external thermocouples are in direct contact to the specimen’s surfaces (figure 4) and therefore measure the exact and “true” surface temperatures (figure 5).

Instrumentation kit featuring orange interface layers and external thermocouples for precision temperature measurement.
3) Instrumentation Kit: Interface layers and external thermocouples
Pyrex® sample with an external thermocouple installed in the center, designed for temperature analysis in testing applications.
4) Pyrex® sample with installed external thermocouple
Pyrex® sample showcased in HFM with labeled interface layers and external thermocouples for thermal analysis.
5) Pyrex® sample with Instrumentation Kit inside the HFM

Comparison of Measurement Data on Pyrex® Using the HFM with Instrumentation Kit and LFA Technique

The performance of the Instrumentation Kit is demonstrated with Pyrex®, a homogeneous, chemically stable and wellknown Thermal ConductivityThermal conductivity (λ with the unit W/(m•K)) describes the transport of energy – in the form of heat – through a body of mass as the result of a temperature gradient (see fig. 1). According to the second law of thermodynamics, heat always flows in the direction of the lower temperature.thermal conductivity reference material since the 1960´s with a Thermal ConductivityThermal conductivity (λ with the unit W/(m•K)) describes the transport of energy – in the form of heat – through a body of mass as the result of a temperature gradient (see fig. 1). According to the second law of thermodynamics, heat always flows in the direction of the lower temperature.thermal conductivity of about 1.14 W/(m∙K) at 23°C [1]. 

The reported data were carried out on specimens measuring 300 mm x 300 mm x 20 mm with and without Instrumentation Kit. The calibration of the heat flux sensors was achieved with a NIST certified glass-fiber board (1450D) without instrumentation kit, in accordance with ASTM C 518. Three different Pyrex samples (A, B, C) from the same batch were tested. Two samples (1, 2) with a diameter of 12.7 mm and a thickness of 2.5 mm were also prepared from the same batch for the LFA tests. The measurements were performed with the LFA467 Hyperflash. 

Table 1 shows the results at 23°C from different HFM and LFA tests. The small standard deviation (1.7%) of the HFM tests demonstrates the good reproducibility of the method. The mean Thermal ConductivityThermal conductivity (λ with the unit W/(m•K)) describes the transport of energy – in the form of heat – through a body of mass as the result of a temperature gradient (see fig. 1). According to the second law of thermodynamics, heat always flows in the direction of the lower temperature.thermal conductivity of 1.15 W/(m∙K) shows a deviation of only 0.88% to the mean value from LFA and literature. This proves the accuracy of the HFM measurements with the Instrumentation Kit.

Table 1: Thermal conductivity of Pyrex® at 23°C using HFM and LFA

Method

Sample/Measurement

Thermal ConductivityThermal conductivity (λ with the unit W/(m•K)) describes the transport of energy – in the form of heat – through a body of mass as the result of a temperature gradient (see fig. 1). According to the second law of thermodynamics, heat always flows in the direction of the lower temperature.Thermal Conductivity

W/(m∙K)

Mean Thermal ConductivityThermal conductivity (λ with the unit W/(m•K)) describes the transport of energy – in the form of heat – through a body of mass as the result of a temperature gradient (see fig. 1). According to the second law of thermodynamics, heat always flows in the direction of the lower temperature.Thermal Conductivity

W/(m∙K)

HFMPyrex A1.131.15
Pyrex B1.17
Pyrex C1.14
HFMPyrex without Instrumentation Kit0.530.53
LFAPyrex - 11.141.14
Pyrex - 21.14

Without the Instrumentation Kit, the high thermal Contact ResistanceAccording to the second law of thermodynamics, heat transfer between two systems always moves in the direction from higher to lower temperatures. The amount of thermal energy transferred by heat conduction, e.g., through a wall of a building, is influenced by the thermal resistances of the concrete wall and the insulation layer.contact resistance and the unknown surface temperatures lead to a thermal conductivity of 0.53 W/(m∙K), significantly lower than the expected value. 

Figure 6 depicts results from 10°C to 65°C with the HFM, the LFA and literature values (error bars ± 5%). Over the whole temperature range, the HFM and LFA results are in good agreement with literature values (max. deviation 2.8% – LFA and 3.9% – HFM).

Thermal conductivity vs. temperature graph for Pyrex®, showing measured values with comparison to literature data.
6) Thermal ConductivityThermal conductivity (λ with the unit W/(m•K)) describes the transport of energy – in the form of heat – through a body of mass as the result of a temperature gradient (see fig. 1). According to the second law of thermodynamics, heat always flows in the direction of the lower temperature.Thermal Conductivity of Pyrex® from 10°C to 65°C measured with HFM and LFA compared to literature values

Summary

The thermal conductivity of stiff materials up to 2 W/(m∙K) can be reliably investigated with the HFM, provided that the surface temperatures are accurately measured. This is achieved with the Instrumentation Kit, which ensures a homogeneous heat flow and true specimen´s surface temperatures. The data of the HFM measurements with the Instrumentation Kit are highly reproducible and in good agreement with the results from the LFA technique and literature. Furthermore, the long term stability qualifies Pyrex® as a material of choice for verifying the performance of the HFM with Instrumentation Kit prior to measuring unknown, high conductive samples.

Literature

  1. [1]
    I. Williams, R. E. Shawyer: Certification report for a pyrex glass reference material for thermal conductivity between-75°C and 195°C; Commission of the European Communities; Luxembourg; 1991