Published on 

Skutterudite: High-Performance Material for Thermoelectric Applications

The Importance of Thermoelectric Materials and Their Application Possibilities

The optimization of energy efficiency is one of the major challenges of the 21st century. In many industrial applications, huge amounts of unused thermal energy are generated. Such waste heat is produced by melting furnaces, incineration plants, power plants and even motor vehicles – and could all be used for the generation of electrical energy. Along with having a positive environmental impact, this would also contribute significantly to increasing the overall efficiency and profitability of industrial plants. That’s where thermoelectrics come into play.

“Thermoelectric generators”, as they are known, are developed and can be employed in all areas where usable temperature differences are available. Such applications require the development of thermoelectric materials with high efficiency.

Determination of Thermophysical and Thermoelectric Properties

For the development and optimization of thermoelectric materials, knowledge of the thermophysical and thermoelectric properties is essential. For assessment of the efficiency, the figure of merit (ZT value) is used. This thermoelectric figure describes how well or poorly suited a special material is for use in a thermoelectric generator. The ZT value thus yields information on the material’s efficiency.

Mathematical equations for thermoelectric performance, showcasing ZT and λ parameters, critical for material analysis.

With the Electrical Conductivity (SBA)Electrical conductivity is a physical property indicating a material's ability to allow the transport of an electric charge.SBA 458 Nemesis®, the Seebeck coefficient, S, and Electrical Conductivity (SBA)Electrical conductivity is a physical property indicating a material's ability to allow the transport of an electric charge.electrical conductivity, σ, can be determined simultaneously. Using the LFA, the Specific Heat Capacity (cp)Heat capacity is a material-specific physical quantity, determined by the amount of heat supplied to specimen, divided by the resulting temperature increase. The specific heat capacity is related to a unit mass of the specimen.specific heat capacity, cp, and Thermal DiffusivityThermal diffusivity (a with the unit mm2/s) is a material-specific property for characterizing unsteady heat conduction. This value describes how quickly a material reacts to a change in temperature.thermal diffusivity, a, can be measured directly. Along with the DensityThe mass density is defined as the ratio between mass and volume. density, ρ, the Thermal ConductivityThermal conductivity (λ with the unit W/(m•K)) describes the transport of energy – in the form of heat – through a body of mass as the result of a temperature gradient (see fig. 1). According to the second law of thermodynamics, heat always flows in the direction of the lower temperature.thermal conductivity, λ, can be calculated.

With the Electrical Conductivity (SBA)Electrical conductivity is a physical property indicating a material's ability to allow the transport of an electric charge.SBA 458 Nemesis® and the laser flash apparatuses LFA 427, LFA 457 and LFA 467, NETZSCH offers a complete solution for determination of the ZT value.

Skutterudite as an Appropriate Material for Thermoelectric Applications

Currently, the enormous costs for development and the presently low efficiency of thermoelectric materials often prevent their application. To overcome this, the efficiency of thermoelectrics must be significantly increased via new developments and modifications.

The objective is to develop materials exhibiting low Thermal ConductivityThermal conductivity (λ with the unit W/(m•K)) describes the transport of energy – in the form of heat – through a body of mass as the result of a temperature gradient (see fig. 1). According to the second law of thermodynamics, heat always flows in the direction of the lower temperature.thermal conductivity, λ, with simultaneously high conductivity, σ, and a high Seebeck coefficient, S. The difficulty here is in the fact that these three properties can only be influenced independently of one another under certain conditions.

Skutterudite in particular has the potential for excellent electrical properties. Skutterudite is a material consisting of cobalt and arsenic, often contaminated by rare earths. It belongs to the class of sulfides. It owes its name to the city of Skutterud in Norway, which is where this naturally occurring mineral, CoAs3, was first discovered in 1928. It was only in the mid-50s that its excellent electrical properties were recognized. Skutterudite features a very high charge carrier mobility and a medium-sized Seebeck coefficient. Its Thermal ConductivityThermal conductivity (λ with the unit W/(m•K)) describes the transport of energy – in the form of heat – through a body of mass as the result of a temperature gradient (see fig. 1). According to the second law of thermodynamics, heat always flows in the direction of the lower temperature.thermal conductivity, on the other hand, is far too high to have made its efficient use in thermoelectrical applications possible at that point in time. In the 70s, the crystal structure typical for skutterudite was discovered, which can be modified optimally. Two voids in the elementary cell can be filled by the insertion of foreign atoms. This way, the Thermal ConductivityThermal conductivity (λ with the unit W/(m•K)) describes the transport of energy – in the form of heat – through a body of mass as the result of a temperature gradient (see fig. 1). According to the second law of thermodynamics, heat always flows in the direction of the lower temperature.thermal conductivity of skutterudite can be reduced. Since then, skutterudites have been potential candidates for more efficient thermoelectric converters with which, for example, waste heat from the exhaust systems of automobiles could be directly converted into electricity. The following measurement examples show how the ZT value of skutterudite can be determined by means of a single sample.

LFA Measurements

For calculation of the dimensionless ZT value of skutterudite, the Thermal DiffusivityThermal diffusivity (a with the unit mm2/s) is a material-specific property for characterizing unsteady heat conduction. This value describes how quickly a material reacts to a change in temperature.thermal diffusivity (figure 1, red curve) and the Specific Heat Capacity (cp)Heat capacity is a material-specific physical quantity, determined by the amount of heat supplied to specimen, divided by the resulting temperature increase. The specific heat capacity is related to a unit mass of the specimen.specific heat capacity (figure 1, black curve) were determined with the LFA 467 HyperFlash® on a sample with a diameter of 12.7 mm. The measurements were carried out between room temperature and 400°C.

Graph illustrating thermal diffusivity (red curve) and specific heat capacity (black curve) versus temperature in °C.
1) Measurement of the Thermal DiffusivityThermal diffusivity (a with the unit mm2/s) is a material-specific property for characterizing unsteady heat conduction. This value describes how quickly a material reacts to a change in temperature.thermal diffusivity (red curve) and the Specific Heat Capacity (cp)Heat capacity is a material-specific physical quantity, determined by the amount of heat supplied to specimen, divided by the resulting temperature increase. The specific heat capacity is related to a unit mass of the specimen.specific heat capacity (black curve) with the LFA method

Calculation of the Thermal ConductivityThermal conductivity (λ with the unit W/(m•K)) describes the transport of energy – in the form of heat – through a body of mass as the result of a temperature gradient (see fig. 1). According to the second law of thermodynamics, heat always flows in the direction of the lower temperature.thermal conductivity is based on the results obtained by means of the following equation: λ = a·cp·ρ (see figure 2).

Graph depicting thermal conductivity (λ) in MW/mK against temperature (°C), showing a stable trend from 0 to 400°C.
2) Determination of the thermal conductivity

ZT Value

The ZT value is calculated by means of the results obtained with the LFA and Electrical Conductivity (SBA)Electrical conductivity is a physical property indicating a material's ability to allow the transport of an electric charge.SBA on the same sample (see figure 4) using the following equation:

Formula for ZT calculation in thermoelectric material analysis: ZT = (S²σ/λ)T, highlighting key variables for performance testing.
Black circular sample for LFA and SBA measurements, highlighting the simplicity of sample preparation in analysis.
4) Only one sample needs to be used for both the LFA and SBA measurements. There is no need for any additional sample preparation to adjust sample geometry.

The plot in figure 5 represents the increase in ZT value between room temperature and 400°C with a maximum at 0.75.

Graph depicting the increase of the Figure of Merit ZT from 0.2 to 0.75 as temperature rises from room temperature to 500°C.
5) Increase in ZT value between room temperature and 500°C. The maximum is at 0.75.