Published on 

LFA Measurements on Cast Iron into the Molten State

Sample Holder for “Liquid Metals”* (Sapphire)

Reduced development times and costs, optimization of manufacturing processes and lower masses in spite of increasingly higher demands on thermally stressed components are important goals of the automotive industry. For example, numerical simulations are used to predict the temperature distribition within the engine components during the casting process.

A basic necessity for this is the knowledge of the thermophysical properties of the casting material over the entire temperature range. In this application note, the results for the measurement of the thermophysical properties of cast iron are presented. The LFA measurements were carried out using a special sapphire container for measurements on “liquid metals”*. The sapphire container ensures defined dimensions of the liquid.

*In this context, the term „liquid metals“ refers to sample holders that facilitate measurements at temperatures exceeding the Melting Temperatures and EnthalpiesThe enthalpy of fusion of a substance, also known as latent heat, is a measure of the energy input, typically heat, which is necessary to convert a substance from solid to liquid state. The melting point of a substance is the temperature at which it changes state from solid (crystalline) to liquid (isotropic melt).melting point of metals.

Measurement Conditions

Results

The Thermal DiffusivityThermal diffusivity (a with the unit mm2/s) is a material-specific property for characterizing unsteady heat conduction. This value describes how quickly a material reacts to a change in temperature.thermal diffusivity and specific heat (measured with a DSC) show a typical behavior with peaks at the Curie transition (2nd order Phase TransitionsThe term phase transition (or phase change) is most commonly used to describe transitions between the solid, liquid and gaseous states.phase transition). The Thermal ConductivityThermal conductivity (λ with the unit W/(m•K)) describes the transport of energy – in the form of heat – through a body of mass as the result of a temperature gradient (see fig. 1). According to the second law of thermodynamics, heat always flows in the direction of the lower temperature.thermal conductivity decreases nearly continuously up to the melt. A typical step in the Thermal DiffusivityThermal diffusivity (a with the unit mm2/s) is a material-specific property for characterizing unsteady heat conduction. This value describes how quickly a material reacts to a change in temperature.thermal diffusivity/conductivity was detected for the Phase TransitionsThe term phase transition (or phase change) is most commonly used to describe transitions between the solid, liquid and gaseous states.phase transition (solid/liquid) above 1150°C. The reason is that the lattice structure collapses during the Phase TransitionsThe term phase transition (or phase change) is most commonly used to describe transitions between the solid, liquid and gaseous states.phase transition. The example clearly demonstrates that the LFA method is not limited to solid materials with defi ned dimensions. Using the sample holder for liquid metals, the measurement of iron alloys is possible also within the liquid phase.

The example clearly demonstrates that the LFA method is not limited to solid materials with defined dimensions. Using the sample holder for “liquid metals”, the measurement of iron alloys is possible also within the liquid phase.

Thermal analysis graph for cast iron showing thermal diffusivity, conductivity, and specific heat across varying temperatures.
1) LFA results for cast iron, red: Thermal DiffusivityThermal diffusivity (a with the unit mm2/s) is a material-specific property for characterizing unsteady heat conduction. This value describes how quickly a material reacts to a change in temperature.thermal diffusivity; blue: Thermal ConductivityThermal conductivity (λ with the unit W/(m•K)) describes the transport of energy – in the form of heat – through a body of mass as the result of a temperature gradient (see fig. 1). According to the second law of thermodynamics, heat always flows in the direction of the lower temperature.thermal conductivity; black: specific heat