17.05.2021 by Dr. Natalie Rudolph, Dr. Stefan Schmölzer

How Fillers Affect the Crystallization Behavior of SLS Powders

Due to the still limited number of available materials for the Selective Laser Sintering process, there is a constant demand for materials with different properties. The addition of any filler to SLS powder typically has an effect on the processing behavior. Today, we investigate the CrystallizationCrystallization is the physical process of hardening during the formation and growth of crystals. During this process, heat of crystallization is released.crystallization behavior of PA12 powder filled with copper spheres and flakes.

One demand could be higher ductility (e.g., PA11), others could be better dimensional stability (e.g., addition of glass beads), higher electrical or Thermal ConductivityThermal conductivity (λ with the unit W/(m•K)) describes the transport of energy – in the form of heat – through a body of mass as the result of a temperature gradient (see fig. 1). According to the second law of thermodynamics, heat always flows in the direction of the lower temperature.thermal conductivity (e.g., fillers such as aluminum or copper) or increased stiffness and strength (e.g., addition of glass or carbon fibers). 

Fillers act as nucleation sites

The addition of any filler to SLS powder typically has an effect on the CrystallizationCrystallization is the physical process of hardening during the formation and growth of crystals. During this process, heat of crystallization is released.crystallization behavior as the surfaces of the fillers act as heterogeneous nucleation sites. Conductive fillers can also affect the material temperature and therefore, show additionally changed behavior. Dynamic Differential Scanning Calorimetry (DSC) measurements can provide a first indication of a changed behavior, which can then be further analyzed through IsothermalTests at controlled and constant temperature are called isothermal.isothermal measurements at or close to the build temperature. 

Adding conductive copper fillers

To understand the effect of conductive fillers, researchers at the Institute of Polymer Technology (LKT) at the University of Erlangen-Nuremburg experimented with copper fillers [1]. They used different mixtures of copper spheres and flakes (Figure 1) in varying contents and analyzed the processing behavior as well as the resulting conductive properties with the aim to generate complex components for thermal management. A variety of samples were prepared by adding copper spheres in 5 and 10 vol% and copper flakes at 5 vol% to the PA12 powder. The energy DensityThe mass density is defined as the ratio between mass and volume. density of 0.043 J/mm2 was kept constant for all materials to detect any changes in the process behavior due to the fillers.

Figure 1: Scanning Electron Microscope images of copper flakes and spheres [1]

Determining the process window and crystallization behavior of PA12 powder with copper particles

At NETZSCH Analyzing & Testing, a DSC 214 Polyma was used to analyze the process window and the CrystallizationCrystallization is the physical process of hardening during the formation and growth of crystals. During this process, heat of crystallization is released.crystallization behavior of these different mixtures of PA12 powder with copper particles in comparison to the neat PA12 material. 

For each measurement, a sample of 5 mg was cut and placed into an aluminum pan with concave bottom (Concavus®® Al) and closed lid. The sample was cooled from room temperature to start the measurement at -20°C. It was then heated to 200°C at a heating rate of 10 K/min and cooled down at the same cooling rate of 10 K/min to -20°C.

The following table summarizes the measurement conditions.

Table 1: Measurement conditions  

Pan Concavus®® Al, closed lid 
Sample weight 5 mg 
Atmosphere N2 
Temperature range -20°C to 200°C at a heating and cooling rate of 10 K/min 

The results for the neat PA12 were discussed in detail in this previous blogpost!

Changes in crystallization behavior

In Figure 2, the results of the 1st heating and cooling are depicted for all 4 samples. As can be seen, the peak Melting Temperatures and EnthalpiesThe enthalpy of fusion of a substance, also known as latent heat, is a measure of the energy input, typically heat, which is necessary to convert a substance from solid to liquid state. The melting point of a substance is the temperature at which it changes state from solid (crystalline) to liquid (isotropic melt).melting temperature is not affected by the addition of the fillers (The difference in area is related to the varying filler contents and was not normalized in this graph).

Figure 2: 1st heating and cooling of PA12 SLS parts at a heating and cooling rate of 10 K/min

However, it can be seen that the peak CrystallizationCrystallization is the physical process of hardening during the formation and growth of crystals. During this process, heat of crystallization is released.crystallization temperature as well as the onset of CrystallizationCrystallization is the physical process of hardening during the formation and growth of crystals. During this process, heat of crystallization is released.crystallization are shifted to higher temperatures with increasing filler content.

The peak is shifted from 145.8°C for the neat material to 149.1°C for 5 vol% copper fillers and to 151.3°C for 10 vol%, respectively.

It can be concluded that the fillers act as nucleation sites and accelerate CrystallizationCrystallization is the physical process of hardening during the formation and growth of crystals. During this process, heat of crystallization is released.crystallization. This leads to a slightly reduced process window and needs to be taken into account during the selection of the processing conditions.

A similar effect was observed by the WILO SE, a premium provider of pumps and pump systems, for glass and carbon fibers. Read the case study here!

Getting a better understanding of the crystallization behavior

Additional studies of the IsothermalTests at controlled and constant temperature are called isothermal.isothermal CrystallizationCrystallization is the physical process of hardening during the formation and growth of crystals. During this process, heat of crystallization is released.crystallization behavior can be useful to understand this behavior even better. A detailed description of the measurement procedure is given here for unfilled PA12 powder.

The researchers at LKT performed these additional isothermal studies at 165°C on the copper filled samples and found that the CrystallizationCrystallization is the physical process of hardening during the formation and growth of crystals. During this process, heat of crystallization is released.crystallization half time is reduced due to the addition of fillers, further confirming the nucleation effect. The whole study can be found here [Open Access]!

About the Institute of Polymer Technology (LKT)

The Institute of Polymer Technology is an academic research institute at the Friedrich-Alexander University of Erlangen-Nuremberg. It is one of the leaders in Additive Manufacturing research; particularly SLS. Other main research areas include Lightweight Design and FRP, Materials and Processing, Joining Technology and Tribology. In addition to these research focuses, the institute is also working on cross-disciplinary topics such as Filler Material ­Compounding, Simulation of Processing and Applications, Radiation Cross-linked Thermoplastics, Gentle Processing and many more.

Sources

[1] Lanzl, L., Wudy, K., Greiner, S., Drummer D., Selective Laser SinteringSintering is a production process for forming a mechanically strong body out of a ceramic or metallic powder. Sintering of Copper Filled Polyamide 12: Characterization of Powder Properties and Process Behavior, Polymer Composites, pp. 1801-1809, 2019.