Assessing the Dispersion Stability Using Creep Testing on a Rotational Rheometer – Shower Gels

Introduction

Whether the long-term stability of an emulsion or suspension is governed by a zero shear viscosity or a Yield StressYield stress is defined as the stress below which no flow occurs; literally behaves like a weak solid at rest and a liquid when yielded.yield stress is dependent upon its microstructure. Furthermore, it is the state of this microstructure at long timescales that is important since this is ultimately what any dispersed phase will encounter over prolonged storage. One way to determine the existence, and if so magnitude of this low shear (zero shear) viscosity is from a CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep test. This test involves applying a constant StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress over a prolonged timescale and monitoring the resultant StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain or compliance (StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain/StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress) as a function of time.

As shown in Figure 1, a purely viscous material will show a constant increase in compliance with time indicative of flow, i.e., steady state viscous response. In contrast, a solid will show a zero gradient indicating an elastic response.

Creep testing principles illustrate the responses of elastic, viscous, and viscoelastic materials under shear stress over time.
1) Principle of CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep testing for an (a) elastic; (b) viscous; (c) viscoelastic materials

For viscoelastic materials, the response will be a combination of viscous and elastic effects as shown in Figure 2, with the response at long times indicating whether it has a Yield StressYield stress is defined as the stress below which no flow occurs; literally behaves like a weak solid at rest and a liquid when yielded.yield stress (elastic) or a steady state viscous response (viscous). If the material shows a steady-state viscous response, then the zero shear viscosity is simply given by the inverse gradient of the compliance versus time plot.

Graph comparing creep responses of a viscoelastic liquid (blue) and a viscoelastic solid (red) over time.
2) CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.Creep response for a viscoelastic liquid (blue) and a viscoelastic solid (red)

If the average particle size, DensityThe mass density is defined as the ratio between mass and volume. density and volume fraction of the dispersed phase are known, and the zero shear viscosity of the continuous phase is determined, then the velocity (V) of the dispersed phase can be estimated using the following modification of Stokes equation:

TCC 918 Cone Calorimeter, a fire testing instrument for measuring heat release and smoke development in materials.
Equation 1 [1]

a = the particle radius (sphere)
Δρ = the DensityThe mass density is defined as the ratio between mass and volume. density difference between particle and liquid
η = the viscosity of the liquid (zero shear viscosity)
g = acceleration due to gravity
φ = the phase volume

The value of the exponent is generally 4.75 for a radius >1 μm and 5.25 for a radius <1 μm.

Potentially, the dispersion can then be re-formulated to obtain a low shear viscosity sufficient to suspend the dispersed phase for the required period, or alternatively to introduce a Yield StressYield stress is defined as the stress below which no flow occurs; literally behaves like a weak solid at rest and a liquid when yielded.yield stress which would give a solid-like response at long times.

It is important when running a CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep test that sufficient time is allowed for steady state to be reached. If not, then too low a value of the zero shear viscosity may be reported or indeed an incorrect assumption is made that the material has a zero shear viscosity when it actually has a Yield StressYield stress is defined as the stress below which no flow occurs; literally behaves like a weak solid at rest and a liquid when yielded.yield stress. Since dispersions may sit on a shelf undisturbed for weeks or even months at a time, then this needs to be considered in any test protocol.

This application note shows methodology and data from CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep testing for two commercial shower gel products.

Experimental

Results and Discussion

Figure 3 shows the CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep response for the two shower gel products on a logarithmic scale. Clearly the two products show a similar initial elastic response, however, there are differences in the delayed elastic response as indicated by the timescale required to achieve steady state. The steady state tolerance range employed in this test was within ± 1% for 60 seconds. Clearly sample A displays steady state behavior almost immediately, while Sample B has some residual elasticity.

Log compliance plots for two shower gel products, Sample A in red and Sample B in blue, over test time.
3) Plots of log compliance against test time for the two shower gel products

Figure 4 shows the same plot but using a linear scale. This makes it easier to distinguish the differences in the gradient of the compliance versus time plots. Since η0 is given by the inverse gradient of the steady state portion of the curve then it is clear that sample B will have a higher zero shear viscosity than sample A. These values were automatically calculated as part of the test and were found to be 6 Pas and 12 Pas for sample A and B, respectively. According to Equation 1, this means that sample B would reduce the rate of sedimentation by a factor of 2 for suspensions of equivalent particles and volume fractions. Whether these viscosity values are sufficient to give effective stability will depend on the specific size, DensityThe mass density is defined as the ratio between mass and volume. density and volume of the dispersed phase, which need to be determined using independent techniques.

DSC curves for HDPE sample at varying heating rates show thermal transitions at specific temperatures. Data table highlights similarities.
4) Plots of compliance against test time for the two shower gel products

Conclusions

CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.Creep testing is an effective means of determining the zero shear viscosity of a material and can be used to assess suspension stability.

In this test, it has been shown that a small amount of an associative thickener can double the zero shear viscosity of a surfactant-based shower gel and reduce the rate of sedimentation by a factor of two (for suspensions of equivalent particles and volume fractions).

1Please note that a parallel plate geometry or a cylindrical geo-metry can also be used. The use of a solvent trap is also recommended for these tests since evaporation of solvent (e.g., water) around the edges of the measuring system can invalidate the test, particularly when working at higher temperatures.

Literature

  1. [1]
    Barnes, H A, ´The 1992 IChemE Research Event`, pp