Thermal and Rheological Characterization of Nail Gel Curing

Introduction

From transparent to black, including all the colors of the rainbow, the market of nail gels (those that cure) and nail polishes (those that air dry) offers a wide variety of products. Even if the first selection criteria is often an aesthetic one, the consumer also wants a product that is practical to apply giving the desired finish and performance. For that, the perfect nail gel or polish should feel relatively liquid for an easy brush application but without flowing outside the nail. The drying or Curing (Crosslinking Reactions)Literally translated, the term “crosslinking“ means “cross networking”. In the chemical context, it is used for reactions in which molecules are linked together by introducing covalent bonds and forming three-dimensional networks.curing time should be as low as possible and lead to a smooth surface for a flawless appearance. Finally, it is also desirable for the manicure to be long-lasting, without it being too difficult to remove. 

Some types of nail gels require a UV-lamp for Curing (Crosslinking Reactions)Literally translated, the term “crosslinking“ means “cross networking”. In the chemical context, it is used for reactions in which molecules are linked together by introducing covalent bonds and forming three-dimensional networks.curing. These products contain a photo-initiator that will initiate the Curing (Crosslinking Reactions)Literally translated, the term “crosslinking“ means “cross networking”. In the chemical context, it is used for reactions in which molecules are linked together by introducing covalent bonds and forming three-dimensional networks.curing reaction as soon as the gel is in contact with the suitable wavelengths emitted by the lamp.

The exposure time, the wavelength and the intensity of the lamp is of great importance for the nail gel to cure in the correct way.

Experimental

The UV Curing (Crosslinking Reactions)Literally translated, the term “crosslinking“ means “cross networking”. In the chemical context, it is used for reactions in which molecules are linked together by introducing covalent bonds and forming three-dimensional networks.curing of three nail gels was characterized by two different methods: 

The sample colors were red, black and clear. The clear sample contained suspended glitters. 

Table 1 summarizes the conditions under which the three different samples were tested.

Table 1: Measurement Conditions

DSCDeviceDSC 300 Caliris® with H-Module
Sample mass3.0 mg
CrucibleConcavus®® (aluminum, open)
Temperature30°C (IsothermalTests at controlled and constant temperature are called isothermal.isothermal)
AtmosphereNitrogen (20 ml/min)
LampOmnicure® S 2000 (wavelength range: 320 to 500 nm)
Exposure duration180 s
Rotational RheometryDeviceKinexus
GeometryPP8 (Plate/Plate, diameter: 8 mm)
Gap250 μm
Temperature25°C
AtmosphereAmbient (air)
LampOmnicure® S 2000 (wavelength range: 320 to 500 nm)
Exposure duration30 s

DSC – Functional Principle

Based on ISO 11357, heat-flux DSC is a technique in which the difference between the heat flow rate into a sample crucible and that into a reference crucible is determined as a function of temperature and/or time. During such a measurement, the sample and reference are subjected to the same controlled temperature/time program and atmosphere.

Cross-sectional diagram of a differential scanning calorimeter (DSC) showing sample, reference, and thermocouples.

Rotational Rheometry (Oscillation Measurement) – Functional Principle

The upper plate oscillates with a defined frequency f [Hz] (or ω [rad/s]) and amplitude [%] (or shear StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain γ [%]), γ = γo + sin (ωt).

The shear StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress σ [Pa] required for this oscillation is determined: σ = σ0 + sin(ωt+δ).

Result: The viscoelastic properties of the sample are determined, in particular its complex stiffness G* (|G*| in [Pa]).

The “in-phase” part of G* is related to the elastic properties (→ G', storage shear modulus), the “out-phase” part to the viscous properties (→ G'', loss shear modulus) of the viscoelastic material.

Stress-strain relationship graphs illustrating output stress and input strain curves, alongside G' and G'' parameters.

Thermal Analysis and Speed of Curing

Curing effects can be observed in the DSC curves in the form of ExothermicA sample transition or a reaction is exothermic if heat is generated.exothermic effects. The curing reaction can be initiated either by heat or by UV light, when using a DSC equipped with a UV-lamp (photo-DSC). 

Figure 1 depicts the photo-DSC-curves obtained during UV exposure of the three nail gels. The peak area represents the curing enthalpy. The higher the value, the more energy is released during the reaction.

DSC curve analysis of UV curing for black, red, and clear gel with gold glitter nail products, highlighting thermal properties.
1) DSC curve resulting from UV curing of the nail gels

The clear sample containing glitters has the curing peak with the highest reaction enthalpy (211 J/g). That does not mean that it needs more time than the other two to finish the reaction. Actually, it is also the one that reacts most rapidly, as demonstrated by the slope of the curve before the peak maximum is reached: It is the steepest for this material. Figure 2, which depicts the conversion rate for all three samples, illustrates this result. The higher the peak maximum value and the steeper the slope before the peak maximum, the faster the conversion rate. Consequently, curing is fastest for the clear sample with glitters (peak maximum already reached at 11.5 s after exposure to UV light and associated with the highest conversion rate of 7.0%/s). 

In contrast, the black sample exhibits the opposite behavior. The reaction is the slowest (a more gradual slope of the curve before peak maximum, leading to a conversion rate curve with peak maximum of 3.8%/s at 12.3 s) and is associated with the lowest energy release (127 J/g). 

The red nail gel shows a curing behavior between the other two, both for the reaction speed and the curing enthalpy.

Conversion rate graph comparing curing times for three nail gels: clear gel with gold glitters, red gel, and blank gel.
2) Conversion rate of the curing for the three nail gels

Figure 3 displays the Complex ModulusThe complex modulus consists of two components, the storage and the loss moduli. The storage modulus (or Young’s modulus) describes the stiffness and the loss modulus describes the damping (or viscoelastic) behavior of the corresponding sample using the method of Dynamic Mechanical Analysis (DMA). complex modulus curves for all three samples. Before curing, all samples possess a similar stiffness of 70 - 80 Pa. The significant increase in modulus indicates curing has started. Similar to DSC, the slope of the curve is related to the reaction speed. The results correlate to those obtained with DSC: The clear nail gel with glitters cures fastest and the black sample shows the slowest curing of the three samples.

Complex modulus comparison of clear glitter, red, and black nail gels over time, highlighting their varying consistencies.
3) Complex modulus of the three different nail gels

The samples differ also in their final modulus. The modulus of the clear gel with glitters increases by 6 decades during curing, vs. less than 4 decades for the black gel. This means that the clear gel reveals the highest stiffness after curing. 

Additionally, Figure 4 shows the curves of G', G'' and δ during the curing process under UV-light of the black sample. At the beginning of the measurement, the viscous shear modulus (G", blue) is higher than the elastic shear modulus (G', red). The phase angle is high (more than 80°). This means that under these measurement conditions, prior to curing, the nail gel behaves almost like a perfect viscous liquid with only very weak elastic properties.

Graph illustrating the elastic and viscous shear modulus, and phase angle during UV-curing of black nail gel over time.
4) Curves of elastic, viscous shear modulus and phase angle obtained during UV-curing of the black nail gel

The curing reaction leads to an increase of both G' and G''. They crossover 7 seconds after UV exposure. In practice, the crossover means that from this time, the network built through curing is strong enough to prevent flow of the material on the time scale corresponding to 1 Hz. At the end of the measurement, the curves of G' and G" are still increasing, even if this rise is not significant. The exposure to UV-light initiated a curing process that is able to continue despite the lamp being switched off.

Phase Angle

The phase angle δ (δ = G''/G') is a relative measure of the viscous and elastic properties of a material. It ranges from 0° for a fully elastic material to 90° for a fully viscous material.

Does a High Curing Speed Make the Sample Better?

A faster cure is advantageous for the consumer. However, the final properties of the manicure after application are of course also important. A post-cure amplitude sweep helps us predict the behavior of the gels after curing by providing information about their inner structure. 

For that, the linear-viscoelastic region of the two extreme samples (clear with glitters and black) are compared in Figure 5. 

The Linear Viscoelastic Region (LVER)In the LVER, applied stresses are insufficient to cause structural breakdown (yielding) of the structure and hence important micro-structural properties are being measured.LVER-plateau of the black nail gel is wider with a lower modulus than that of the clear sample, indicating that the cured black gel is likely to be more flexible.

Even if the clear nail gels cures faster than the black one, it will also exhibit more brittle properties.

Post-curing amplitude sweep graph comparing the mechanical properties of clear gel with gold glitters and black gel.
5) Post-curing amplitude sweep of the black and clear

Linear Viscoelastic Region (LVER)In the LVER, applied stresses are insufficient to cause structural breakdown (yielding) of the structure and hence important micro-structural properties are being measured.LVER – Linear Viscoelastic Region

Conclusion

DSC and rotational rheometry are two complementary methods for the characterization of the curing of nail gels. 

Both methods highlight the curing speed. The DSC 300 Caliris® additionally provides information about the energy released during curing, while measurements with the Kinexus compare the properties of the different products during and after curing.