Published on 

Rheological Characterization of Artificially Aged Liquid Colors

Method for Characterizing Aging Behavior – A Comparative Study for Evaluating Time-DependentChanges in Liquid Colors When Stored at Room and Elevated Temperatures

Background and Motivation

In many areas of consumer goods, color and design are just as important as the function of a component. Color and its processing in the product, for example, convey a feeling, of quality and value. It serves for identification purposes and points out danger, respect or purity. Due to the increasing demand for color variety, plastic manufacturers directly color the parts during the injection molding process, often using (color) masterbatches. 

Liquid colors are a cost-efficient and flexible alternative to masterbatches for coloring plastic components. In comparison to masterbatches, better dispersion of the pigments in the plastics is a major advantage, leading to lower dosing quantity in order to achieve the same color quality as with masterbatches. In addition, the liquid carrier material, that is based, for example, on unsaturated fatty acid ester or natural oils, yields a cleaning effect in the injection molding machine. This enables faster color changes which significantly reduces the scrap rate. Along with possible impacts on processing (e.g., stick-slip) and the material properties of the finished part (softening effect on the polymer), the storage behavior of liquid colors is also of great interest for the application. 

This application note investigates whether accelerated aging of liquid colors is possible due to an increased storage temperature and whether this is evident from changed rheological properties.

In particular, the following questions should be answered using a simple model system: 

  1. Is it possible to observe changes in liquid colors during storage by rheology? 
  2. Can the occurring changes be accelerated by increasing the storage temperature and can the behavior of liquid colors be predicted?

Material and Methods

Liquid colors are mixtures of substances consisting of a liquid carrier and binder, colorants and additves. Typical carriers are vegetable oils, paraffin oils and fatty acid esters. In addition to inorganic and organic pigments, dyes can be used as colorants. The additives used in liquid colors may be necessary for the formulation and use of the liquid color (e.g., wetting and dispersing additives, defoamers, rheological additives), but also for the performance of the finished product, e.g., for improved UV stability or as flame retardants. 

A simplified model system without additional additives is employed for the investigations. The model system consists of a rapeseed oil as a carrier with sorbitan fatty acid esters (Tween80/Span80 blend) as a binder and Carbon BlackTemperature and atmosphere (purge gas) affect the mass change results. By changing the atmosphere from, e.g., nitrogen to air during the TGA measurement, separation and quantification of additives, e.g., carbon black, and the bulk polymer can become possible.carbon black as the pigment. The solid mass fraction of the Carbon BlackTemperature and atmosphere (purge gas) affect the mass change results. By changing the atmosphere from, e.g., nitrogen to air during the TGA measurement, separation and quantification of additives, e.g., carbon black, and the bulk polymer can become possible.carbon black particles in the model system is 15.5%. The suspensions were stored at both 20°C (room temperature) and 40°C for accelerated aging. In parallel, samples without pigment were aged and analyzed in order to detect possible changes in the carrier system. 

The rheological tests were carried out at different times (after 0, 3, 9, 18, 36, 72 and 150 days) of storage.

Prior to the tests, all samples were stirred and homgenized at moderate/low stirring rates using a dual asymmetric centrifuge. The samples stored at 40°C were subsequently adjusted to the measurement (room) temperature for a minimum of 1 hour. 

Samples were characterized using the NETZSCH rotational rheometer models, Kinexus Prime ultra+ and Kinexus pro+, at 20°C. Preliminary tests have shown that measurements with plate-plate measuring geometries provide comparable results for this material system to those with concentric-cylinder measuring geometries. All samples are investigated with a plate-plate measurement geometry by means of rotational rheology. For the sample stored at 40°C, oscillatory rheological measurements (frequency sweeps) are also performed. The concentric-cylinder measuring geometry was used enabling larger sample volume to be tested. 

While the investigation using rotational rheology was mainly used to detect changes in material behavior, the frequency sweeps were intended to obtain information about the changes in viscoelastic behavior.

Results and Discussion

The viscosity curves of suspensions stored at room temperature are shown on the left in Figure 1, measured at increasing shear rates. A decreasing shear viscosity with increasing shear rates, indicating a Shear ThinningThe most common type of non-Newtonian behavior is shear thinning or pseudoplastic flow, where the fluid vis­cosity decreases with increasing shear.shear-thinning behavior can clearly be seen. Liquid colors are suspensions and when a shear StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress is applied, the particles are aligned in the shear direction, resulting in less resistance to flow. Additionally, at shear rates below 10 s-1, a decrease in shear viscosity is observed with increasing storage time. This can be interpreted that structural degradation is occurring over the storage time. In addition to the measurements shown, rotational measurements were carried out on the rapeseed oil tween-chip samples at the respective time periods. Comparison with the particle-free samples over time revealed both Newtonian behavior and no age-related change in shear viscosity. The method of storage, whether at room temperature or at 40°C, has no effect on the shear viscosity measured and the flow curve of the particle-free samples. It can therefore be assumed that a change in shear viscosity of the rapeseed oil does not explain the changes in shear viscosity of the suspensions.

Viscosity curves of suspensions at room temperature and 40°C, highlighting differences over time in shear rates.
1) Left: Viscosity curves of the suspensions, stored at room temperature and right: Viscosity curves of the suspensions, stored at room temperature and at 40°C. The samples stored at room temperature are highlighted in the legend.

With increasing StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress (>10 s-1), the Shear ThinningThe most common type of non-Newtonian behavior is shear thinning or pseudoplastic flow, where the fluid vis­cosity decreases with increasing shear.shear-thinning effect decreases due to the gradual arrangement of the particles in the flow field. As a result, the difference between the samples at different time intervals (age) also decreases and the measurement curves typically exhibit a similar result. 

After 150 days at room temperature and after 72 days at 40°C, the samples show a deviating tendency, particularly in the higher shear rate range. An increase in shear viscosity can be observed around 10 s-1 compared to the younger samples. As this behavior is already evident after 72 days for the sample stored at 40°C, it can be assumed that the storage time could be reduced by about half for the same changes in the rheological behavior investigated. As shown on the right in Figure 1, a similar tendency can be observed for the suspension stored at 40°C for 72 days. This can be interpreted by hydrodynamic effects like flow-induced liquid immobilization [1] becoming more significant with increasing storage time and the associated possible structural changes. 

Along with the investigation of the dynamic shear viscosity, a frequency sweep measurement was carried out on the suspensions by means of oscillation. This enables mapping of both the elastic and viscous properties, known as the storage and Viscous modulusThe complex modulus (viscous component), loss modulus, or G’’, is the “imaginary” part of the samples the overall complex modulus. This viscous component indicates the liquid like, or out of phase, response of the sample being measurement. loss modulus.

Figure 2 depicts the frequency spectrum between 10 Hz and 10-2 Hz. In line with the shear viscosity measurements already discussed, a decrease in rheological parameters with increasing storage time can again be observed. The storage modulus (G‘) is generally higher than the Viscous modulusThe complex modulus (viscous component), loss modulus, or G’’, is the “imaginary” part of the samples the overall complex modulus. This viscous component indicates the liquid like, or out of phase, response of the sample being measurement. loss modulus (G“), illustrating a solid-dominated material behavior under the conditions tested.

It should be emphasized, however, that a crossover of the storage and Viscous modulusThe complex modulus (viscous component), loss modulus, or G’’, is the “imaginary” part of the samples the overall complex modulus. This viscous component indicates the liquid like, or out of phase, response of the sample being measurement. loss modulus is observed for the suspension stored at 40°C for 75 days and that the Viscous modulusThe complex modulus (viscous component), loss modulus, or G’’, is the “imaginary” part of the samples the overall complex modulus. This viscous component indicates the liquid like, or out of phase, response of the sample being measurement. loss modulus dominates at frequencies > 3 Hz. This can be interpreted as a possible viscosity-dominated behavior for this sample under the given measurement conditions and may indicate that the storage stability of the suspensions is limited. For all suspensions stored for shorter times, however, the Viscous modulusThe complex modulus (viscous component), loss modulus, or G’’, is the “imaginary” part of the samples the overall complex modulus. This viscous component indicates the liquid like, or out of phase, response of the sample being measurement. loss modulus is lower than the storage modulus over the entire frequency range analyzed.

Frequency sweep graph showing storage and loss modulus of samples at 40°C over various time periods, labeled with data points.
2) Frequency sweeps of samples stored at 40°C for different periods of time.

Summary & Outlook

The rheological investigations presented have shown that the liquid colors exhibit Shear ThinningThe most common type of non-Newtonian behavior is shear thinning or pseudoplastic flow, where the fluid vis­cosity decreases with increasing shear.shear-thinning behavior. In addition, it could be observed that the flow behavior of the rapeseed-oil-Carbon BlackTemperature and atmosphere (purge gas) affect the mass change results. By changing the atmosphere from, e.g., nitrogen to air during the TGA measurement, separation and quantification of additives, e.g., carbon black, and the bulk polymer can become possible.carbon black suspensions change with increasing storage time such that the values of the rheological variables investigated decrease. This change can be observed both in the shear viscosity and in the frequency-dependent storage and Viscous modulusThe complex modulus (viscous component), loss modulus, or G’’, is the “imaginary” part of the samples the overall complex modulus. This viscous component indicates the liquid like, or out of phase, response of the sample being measurement. loss modulus. 

By increasing the storage temperature, aging was accelerated in the rapeseed oil-Carbon BlackTemperature and atmosphere (purge gas) affect the mass change results. By changing the atmosphere from, e.g., nitrogen to air during the TGA measurement, separation and quantification of additives, e.g., carbon black, and the bulk polymer can become possible.carbon black suspension. However, it should be noted that other aging mechanisms may be dominant due to the elevated temperature which should be clarified by further investigations. 

Focus of these investigations was to characterize the rapeseed-Carbon BlackTemperature and atmosphere (purge gas) affect the mass change results. By changing the atmosphere from, e.g., nitrogen to air during the TGA measurement, separation and quantification of additives, e.g., carbon black, and the bulk polymer can become possible.carbon black suspensions. In addition, from an applicational point of view, it is of particular interest the processability of liquid colors stored at room temperature and at a temperature of 40°C during injection molding. 

The investigations were carried out on a model system. Finally, it needs to be clarified whether different temperature-time dependencies can be observed for various systems of liquid colors. This will help determine if different temperatures are relevant for artificial aging. It may also be possible to identify classes of liquid colors with comparable aging behavior. Further investigations should also include the determination of the maximum temperature at which artificial aging can be carried out.

Literature

  1. [1]
    Windhab, E. J., 2000, Fluid immobilization – A structure-related key mechanism for the viscous flow behavior of concentrated suspension systems. Applied Rheology, 2002
AI Overview