Creep Behavior of PE-HD under Different Loads and Temperatures

Introduction

When a metal is subjected to a force, it usually deforms immediately and then remains in the same shape even after a long period of time. If the load was not too high, the metal will also return elastically to its original state when the load is removed. When polymers are loaded with a force, they also deform immediately; after a longer period of time, however, it is often found that the body has deformed even further. This behavior is called CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep. Basically, metals also CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep, but with polymers, this behavior is much more pronounced and must be kept in consideration when describing mechanical behavior. For this reason, a quasi-static stress-strain diagram is often sufficient for metals; for polymers, however, the time-dependent deformation should also be taken into account.

Here, it is important to basically distinguish between CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep and RelaxationWhen a constant strain is applied to a rubber compound, the force necessary to maintain that strain is not constant but decreases with time; this behavior is known as stress relaxation. The process responsible for stress relaxation can be physical or chemical, and under normal conditions, both will occur at the same time. relaxation: In CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep, a constant load acts on the body, which consequently deforms. In RelaxationWhen a constant strain is applied to a rubber compound, the force necessary to maintain that strain is not constant but decreases with time; this behavior is known as stress relaxation. The process responsible for stress relaxation can be physical or chemical, and under normal conditions, both will occur at the same time. relaxation, deformation of a body remains constant, but over time, the required force is reduced. RelaxationWhen a constant strain is applied to a rubber compound, the force necessary to maintain that strain is not constant but decreases with time; this behavior is known as stress relaxation. The process responsible for stress relaxation can be physical or chemical, and under normal conditions, both will occur at the same time. Relaxation is of great interest for certain applications, such as for seals; but for many components, it is rather the load that is constant and the time behavior of the deformation that is of interest.

In materials testing, the actual CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep measurement is often combined with a recovery phase (Creep RecoveryCreep recovery is the ratio of the recoverable creep compliance to initial creep compliance given in percent. Often in MSCR (multiple stress creep recovery) testing, creep recovery is considered a performance indicator with more recovery indicating a binder less prone to rutting.creep recovery) in which the material can obtain its original shape again. This way, a distinction can be made between elastic and and irreversible CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep. The irreversible deformation depends to a large extent on temperature and level of load. These relationships will be investigated in more detail in this publication.

Creep Recovery Measurements on PE-HD

The CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep behavior of polymers is investigated here using the example of semi-crystalline high-DensityThe mass density is defined as the ratio between mass and volume. density polyethylene (PE-HD). The samples with dimensions of 55 x 5 x 2 mm are tested with the help of the dynamicmechanical high-load NETZSCH DMA GABO Eplexor® 500 N in tensile mode (figure 1). 

With the Eplexor®, static forces up to 1500 N can be applied in the temperature range from -160°C to +500°C.

Standard tension holder securely gripping PE-HD sample for material testing, featuring metallic clamps and internal measuring components.
1) PE-HD in standard tension holder

Depending on the application range, different tensile sample holders are available: With the standard tensile sample holder, up to 700 N can be applied, depending on the sample. For higher forces, a stronger version up to 1500 N is available. 

Since the dependence of CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep on force is to be investigated in particular, the individual measurements are compared under increasing loads. This way, different load levels can be investigated in a single measurement series without the need for reclamping. 

With this procedure, however, the sample may in principle be deformed before the actual loading step. In order to prevent deviations from the reference geometry from becoming too extensive, no further load increase is carried out here once a StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain of 10% is reached. The measurements are carried out each at a defined sample temperature. At 50°C, five load steps are carried out from 2 to 6 MPa, with 2 waiting hours in order to guarantee that a stable condition can be established in each case. 

At an elevated temperature of 100°C, the load is only increased to 4 MPa as the maximum StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain is reached. 

As shown in figure 2, CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep typically consists of three phases for each loading step. First, the sample is stretched relatively abruptly, followed by visco-elastic CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep. These two processes are typically reversible. Thereafter, the sample rather transforms into a viscous flow (constant StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain rate) and it can clearly be seen that this flow is more pronounced at higher stresses and temperatures. Since this viscous flow is not reversible, a remanent deformation remains even after the subsequent unloading phase. This visco-plastic behavior occurs with increased intensity at higher temperatures and stresses.

Graphs displaying creep-recovery experiments measuring stress and strain at 50°C and 100°C over time.
2) CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.Creep-recovery experiments under different loads and temperatures

In DIN ISO 899 [4], the tensile CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep test for determinattion of the CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep behavior is described. Although is does not specifically address the CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep-recovery experiments employed here, typical evaluations are presented that can also be used for the respective CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep phases. Figures 3 a) and b) thus show the isochronous stress-strain diagrams associated with the above measurements. The StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain is noted for each StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress after a fixed time and entered in the diagram. Since different loads are applied to a sample in this test series, the StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain refers in each case to the state directly before the load step. This presentation is of particular interest for the design of components because the resulting StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain can be read completely analogous to the classical stress-strain diagram for a given load. Typically, the strains are also of interest after much longer time periods than those recorded here. As seen above, mainly the viscous behavior dominates for longer time periods, which will later be discussed in more detail.

As another typical presentation, DIN ISO 899 describes the time-dependent CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep modulus (figures 3 c and d). The reciprocal value of the modulus, i.e., the CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep compliance, is often used instead, but here, the CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep modulus is shown in accordance with the standard. Presentation of the CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep modulus is particularly suited for investigation of the non-linearity of the material. It becomes clear that the higher stresses generally lead to a lower CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep modulus and thus, to higher compliance.

Isochronous stress-strain diagrams for PE-HD at 50°C and 100°C; creep moduli presented at varying stresses over time.
3) a) and b): Corresponding isochronous stress-strain diagrams; c) and d): CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.Creep moduli of PE-HD at different temperatures and stresses

Description of Creep Rates According to Eyring

Polymer CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep is often described by the four-parameter rheological model (figure 4). The model consists of a spring and damping element (Maxwell element) connected in series. The spring can be used to illustrate instantaneous StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain jump and the damper to model the viscous flow. The visco-elastic behavior is described by the parallel spring-damping element. Thus, for each previously performed creep-recovery experiment, a corresponding model can be identified.

Four-parameter rheology model graph showing stress-strain relationships with time, illustrating recoverable and irrecoverable flow.
4) Four-parameter model of rheology

As shown above, the visco-plastic component relevant for long-term creep is mainly caused by viscous flow. The dependence of viscous flow on temperature and StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress can be derived, model-based, from the probabilities that a molecule will overcome a certain obstacle. Details can be found, for example, in [2]. Here, it is stated as a result that, according to this model, the relationship between StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress and temperature depends linearly on the logarithm of the StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain rate. Accordingly, an increase in StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress leads to an exponential increase in StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain rate. 

Shown in figure 5 are the StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain rates determined for the respective stresses. Along with the measurements already presented above, the experiment was additionally carried out at 110°C. At 50°C, the behavior between the StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain rate and StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress is very well described by the model, i.e., there is a largely linear relationship between the StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress and logarithmic StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain rate. At higher temperatures and stresses, further molecular processes are possible, then leading to a bend in the logarithmic StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain rate. 

In the Eyring plot [1], a separate line is recorded for each temperature. In this respect, the plot allows for presenting the extrapolation of the StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain rate for other stresses. It should be noted, however, that there are also more advanced approaches for including an additional time-temperature superposition; see, for example, [3].

Eyring plot illustrating the creep behavior of PE-HD at varying temperatures (50°C, 100°C, 110°C) against strain rate.
5) Eyring plot for the creep of PE-HD

Conclusion

The creep behavior is heavily dependent on temperature and load level. While elastic creep components can even be measured at smaller forces, higher forces and stresses occur in many applications. The DMA GABO Eplexor® allows for the characterization of load-dependent plastic creep in many cases relevant in practice. It is thereby shown that the long-term creep behavior is mainly determined by the viscous flow of the polymer. Exactly this dependence of the StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain rate on the acting StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress can clearly be illustrated in an Eyring plot.

Literature

  1. [1]
    S. Glasstone, K. Laidler and H. Eyring, The theory of rate processes: the kinetics of chemical reactions, viscosity, diffusion and electrochemical phenomena, New York: McGraw-Hill, 1941.
  2. [2]
    J. Rösler, H. Harders und M. Bäker, Mechanisches Verhalten der Werkstoffe, Springer, 2012.
  3. [3]
    Y. C. Bhuvanesh und V. B. Gupta, „Long-term prediction of creep in textile fibres“, Polymer, pp. 2226-2228, 10 1994.
  4. [4]
    DIN EN ISO 899-1:2018-03 Kunststoffe – Bestimmungdes Kriechverhaltens – Teil 1: Zeitstand-Zugversuch, 2018.