Published on 

Overcoming and Quantifying 'Wall Slip' in Measurements Made on a Rotational Rheometer

Introduction

When making shear rheological measurements on structured liquids – in particular suspensions, emulsions or foams – there is a high probability that the measurement may be affected by a phenomenon known as ´wall slip`. Wall slip generally results from a local depletion of the dispersed phase near the geometry walls, effectively forming a lubrication layer at the surface. As a consequence, bulk rheological properties are no longer being accurately measured leading to an underestimation of the true viscosity. 

A similar effect can be observed when measuring solid like materials where there is insufficient friction between the sample and the wall to support the applied StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress. 

Wall slip can be counteracted in a number of ways when testing on a rotational rheometer, most notably by use of roughened or serrated geometries which effectively take the geometry motion into the bulk of the sample and thus maximize samplesample contact at the expense of sample-wall interactions. For cup and bob systems, vanes and splined geometries can be utilized also. 

Figure 2 shows the consequence of slip for a concentrated particle suspension as measured using smooth parallel plates. The apparent ´dog leg` in the flow curve is a familiar characteristic of wall slip which in this case can be largely eliminated by the use of serrated plates. 

For more subtle occurrences of wall slip, it is less easy to confirm its presence unless measurements are made with smooth and serrated or roughened plates, although in many cases, a user may not have both geometry types available for such a comparison.

Serrated parallel plates demonstrating slip reduction with visible actual gap for testing applications.
1) Serrated parallel plates used to minimize slip
Flow curves comparing viscosity for concentrated dispersion with serrated and smooth plates, highlighting rheological differences.
2) Flow curves for a concentrated dispersion with and without serrated plates

 

In such cases, evidence of slip can be obtained by performing StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress controlled measurements at different gaps. If slip occurs, the slip velocity Vs will depend only on the applied shear StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress σ but not on the gap. In contrast, the velocity difference across the sample, which is used to calculate the shear rate will be both gap and shear StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress dependent. Thus by varying the gap h and keeping the StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress σ constant, it is possible to determine the slip velocity and the true shear rate using Equation 1.

Mathematical equation illustrating the relationship between velocity (V), height (h), and apparent strain rate (γ̇app).

V is the velocity of the upper plate
·γapp is the measured shear rate
·γ is the true shear rate

This is done by plotting the measured rate ·γapp against 1/h which sould result in a straight line with gradient 2Vs and intercept γ·.

In some cases, negative values have been observed for the true shear rate and these have been attributed to loading errors, gap accuracy and gap dependent material properties. Consequently, it is preferable to work at larger gaps where any such errors will be minimized.

Experimental

Results and Discussion

Figure 3 shows plots of shear viscosity versus gap. While the shower gel shows a relatively constant viscosity at each gap, the skin cream shows a slight gradient with lower viscosities reported at smaller gaps which can be attributed to wall slip. To estimate the slip velocity, the measured shear rate was plotted against inverse gap in line with Equation 1. A linear model fit (y = mx+ c) was applied to the data with the gradient of the curve equal to 2Vs and the intercept to equal to the true shear rate.

Viscosity vs gap plots comparing skin cream (red) and shower gel (blue), illustrating fluid properties in testing analysis.
3) Viscosity vs gap plots for a skin cream (red) and shower gel (blue)
Plot displaying shear rate vs. 1/gap for skin cream (red line) and shower gel (blue line), illustrating fluid behavior differences.
4) Apparent shear rate vs 1/gap for a skin cream (red) and shower gel (blue)

 

For the skin cream, the slip velocity was estimated to be 1.3 mm/s and the true shear rate 1.016 s-1. This is quite a lot lower than the measured (apparent) shear rate values of between 3-4 s-1 suggesting a significant degree of wall slip. Consequently for future testing, it would be advised to use roughened or serrated plates for this particular sample. 

For the shower gel the slip velocity was estimated to be just 0.08 mm/s with a true shear rate of 0.68 s-1 compared with the apparent value of approximately 0.76 s-1. This difference is within the likely error range associated with the test and therefore, the shower gel can be considered to show no slippage under these measurement conditions.

Conclusion

A shower gel and skin cream were tested at various gaps to assess the slip velocity at the wall-sample interface. The skin cream showed significant wall slip while this was negligible for the shower gel. This test can therefore be used to estimate the degree of slip for a specific material and test condition and indicate whether the use of roughened or profiled geometries is required.

Please note...

that testing is required to be undertaken with a smooth parallel plate geometry combination.