LFA 467 HT HyperFlash: New Sample Holder Dedicated to Metals

Introduction

For LFA measurements, a defined sample thickness is required. The Thermal DiffusivityThermal diffusivity (a with the unit mm2/s) is a material-specific property for characterizing unsteady heat conduction. This value describes how quickly a material reacts to a change in temperature.thermal diffusivity (a) is proportional to the square of the sample thickness (d): a ~ d². This demands high precision to obtain the exact thickness value. In addition, the heat flow through the outer container walls in the axial direction can be critical for sample holders for liquids. Furthermore, measurements on metal melts can destroy the sample holder. In order to address these critical issues, a new sample holder specifically for “liquid metals”* was developed (figure 1). The special design, with some parts made of stainless steel or SiC and inner parts made of sapphire, allows for measurements with excellent IR-detector signals and therefore high precision. The metal is placed in a sapphire crucible which is closed with a sapphire lid on top. The defined sample thickness in the melt is realized by placing additional mass on top of the sapphire lid. This ensures flexible positioning of the lid in terms of height and prevents any damage to the sapphire part resulting from axial thermal expansion of the metal.

*In this context, the term „liquid metals“ refers to sample holders that facilitate measurements at temperatures exceeding the Melting Temperatures and EnthalpiesThe enthalpy of fusion of a substance, also known as latent heat, is a measure of the energy input, typically heat, which is necessary to convert a substance from solid to liquid state. The melting point of a substance is the temperature at which it changes state from solid (crystalline) to liquid (isotropic melt).melting point of metals.

New stainless steel and SiC sample holders for liquid metals, showcasing their distinct designs and components.
1) Design of the new sample holder for “liquid metals”*; stainless steel (order no. LFA46700B96.040-00) and SiC version (LFA46700B96-041-00)

Test Conditions

  • Material: Aluminum alloy
  • Instruments: LFA 467 HT HyperFlash/DSC 404 F1 Pegaus
  • Temperature range: 450°C → 750°C → 450°C 
  • Sample holder: For liquids and metals; made of sapphire; in SiC version, stainless steel (up to 750°C) and SiC version (up to 1250°C) 
  • Temperature range: 450°C → 750°C → 450°C
  • Sample thickness: 1.5 mm
  • Sample surface preparation: Thin graphite coating

Measurement Results

The suitability of the new sample holder for liquids in conjunction with the LFA 467 HT was checked by means of a series of measurements on an aluminum alloy. Prior to the LFA test, additional DSC measurements were conducted. Figure 2 depicts the Phase TransitionsThe term phase transition (or phase change) is most commonly used to describe transitions between the solid, liquid and gaseous states.phase transition during heating and cooling in the DSC. During heating (black curve), multi-step melting of the alloy starts at 558°C (onset, solidus temperature) with peak temperatures at 569°C and 600°C. The last step is finished at 623°C (liquidus temperature). A slight sub-cooling effect can be seen in the cooling cycle (dashed green line). The crystallizing process starts between 610°C and 600°C, approximately 10–15 K below the liquidus temperature determined during heating. The CrystallizationCrystallization is the physical process of hardening during the formation and growth of crystals. During this process, heat of crystallization is released.crystallization ends at 535°C.

Graph illustrating specific heat capacity of a sample aluminum alloy during heating and cooling, highlighting critical temperature peaks.
2) Specific Heat Capacity (cp)Heat capacity is a material-specific physical quantity, determined by the amount of heat supplied to specimen, divided by the resulting temperature increase. The specific heat capacity is related to a unit mass of the specimen.Specific heat capacity including energetic effects of aluminum alloy during heating (solid black line) and cooling (dashed green line; DSC measurement).

Depicted in figure 3 is the Thermal DiffusivityThermal diffusivity (a with the unit mm2/s) is a material-specific property for characterizing unsteady heat conduction. This value describes how quickly a material reacts to a change in temperature.thermal diffusivity of the aluminum alloy during heating and cooling (LFA measurements). The values during melting and CrystallizationCrystallization is the physical process of hardening during the formation and growth of crystals. During this process, heat of crystallization is released.crystallization are in very good agreement, which indicates that the IR detector has excellent signal stability and that conditions are stable both within and outside of the Phase TransitionsThe term phase transition (or phase change) is most commonly used to describe transitions between the solid, liquid and gaseous states.phase transitions (e.g., constant thickness of liquid/solid metal film). The solidus temperature is detected between 550°C and 575°C (by comparison, DSC: 558°C) and the liquidus temperature between 600°C and 625°C (by comparison, DSC: 623°C). The good agreement between the two independent instruments demonstrates the high temperature accuracy of the LFA 467 HT.

Graph displaying thermal diffusivity of aluminum alloy during heating and cooling phases, highlighting transitions between solid and liquid states.
3) Thermal DiffusivityThermal diffusivity (a with the unit mm2/s) is a material-specific property for characterizing unsteady heat conduction. This value describes how quickly a material reacts to a change in temperature.Thermal diffusivity of aluminum alloy for the Phase TransitionsThe term phase transition (or phase change) is most commonly used to describe transitions between the solid, liquid and gaseous states.phase transitions solid → liquid and liquid → solid.

The calculation of Thermal ConductivityThermal conductivity (λ with the unit W/(m•K)) describes the transport of energy – in the form of heat – through a body of mass as the result of a temperature gradient (see fig. 1). According to the second law of thermodynamics, heat always flows in the direction of the lower temperature.thermal conductivity λ(T) is based on following equation:

λ(T) = ρ(T) · Specific Heat Capacity (cp)Heat capacity is a material-specific physical quantity, determined by the amount of heat supplied to specimen, divided by the resulting temperature increase. The specific heat capacity is related to a unit mass of the specimen.cp(T) · α(T)

where 
ρ = DensityThe mass density is defined as the ratio between mass and volume. density
α = Thermal DiffusivityThermal diffusivity (a with the unit mm2/s) is a material-specific property for characterizing unsteady heat conduction. This value describes how quickly a material reacts to a change in temperature.thermal diffusivity
cp = Specific Heat Capacity (cp)Heat capacity is a material-specific physical quantity, determined by the amount of heat supplied to specimen, divided by the resulting temperature increase. The specific heat capacity is related to a unit mass of the specimen.specific heat capacity

The DensityThe mass density is defined as the ratio between mass and volume. density, ρ, can be determined at room temperature by volume and mass. For precise results, a dilatometer can be used to consider for the thermal expansion and DensityThe mass density is defined as the ratio between mass and volume. density change depending on temperature. The measured/calculated cp*(T) DSC curves contain the contribution of the phase change enthalpies Δhphase and can be described as:

cp* dT = cp dT + dhphase

In order to get the “true” Specific Heat Capacity (cp)Heat capacity is a material-specific physical quantity, determined by the amount of heat supplied to specimen, divided by the resulting temperature increase. The specific heat capacity is related to a unit mass of the specimen.specific heat capacity cp(T) which is needed for the calculation of Thermal ConductivityThermal conductivity (λ with the unit W/(m•K)) describes the transport of energy – in the form of heat – through a body of mass as the result of a temperature gradient (see fig. 1). According to the second law of thermodynamics, heat always flows in the direction of the lower temperature.thermal conductivity, the phase change enthalpy must be subtracted:

cp dT = cp* dT - dhphase

That will usually be done by linear interpolation over the range of Phase TransitionsThe term phase transition (or phase change) is most commonly used to describe transitions between the solid, liquid and gaseous states.phase transition.

Figure 4 presents the thermophysical properties of the aluminum alloy including the calculated Thermal ConductivityThermal conductivity (λ with the unit W/(m•K)) describes the transport of energy – in the form of heat – through a body of mass as the result of a temperature gradient (see fig. 1). According to the second law of thermodynamics, heat always flows in the direction of the lower temperature.thermal conductivity for the solid-liquid Phase TransitionsThe term phase transition (or phase change) is most commonly used to describe transitions between the solid, liquid and gaseous states.phase transition.

NETZSCH DSC 214 Polyma differential scanning calorimeter, featuring an intuitive interface for precise thermal analysis.
4) Thermophysical properties of aluminum alloy for the Phase TransitionsThe term phase transition (or phase change) is most commonly used to describe transitions between the solid, liquid and gaseous states.phase transition solid → liquid.

Summary

NETZSCH developed a new sample holder for “liquid metals”* for the LFA 467 HT HyperFlash® which can be delivered in two versions, usable up to 750°C and 1250°C, respectively. Measurements on a liquid aluminum alloy clearly demonstrate the high reproducibility of the results during heating (melting) and cooling (CrystallizationCrystallization is the physical process of hardening during the formation and growth of crystals. During this process, heat of crystallization is released.crystallization). The special design of the sample holder ensures constant sample thickness during the melt. At the same time, it prevents mechanical pressure on sapphire parts resulting from thermal expansion. Thanks to the excellent signal stability, high precision with low scattering was achieved. Furthermore, good agreement with DSC results was obtained and the detected Phase TransitionsThe term phase transition (or phase change) is most commonly used to describe transitions between the solid, liquid and gaseous states.phase transition temperatures were all in the expected range.

*In this context, the term „liquid metals“ refers to sample holders that facilitate measurements at temperatures exceeding the Melting Temperatures and EnthalpiesThe enthalpy of fusion of a substance, also known as latent heat, is a measure of the energy input, typically heat, which is necessary to convert a substance from solid to liquid state. The melting point of a substance is the temperature at which it changes state from solid (crystalline) to liquid (isotropic melt).melting point of metals.