Evaluating Product Texture Using Oscillatory Testing on a Rotational Rheometer

Introduction

Formulating products to have both the correct functional and sensory attributes can be a difficult task. The latter in particular relies heavily on user feedback, which can take considerable time and effort to attain. In addition, it is not always easy to interpret such feedback in the context of material properties and hence rheological data. 

To use rheology as a tool for evaluating product texture, it is important to understand which rheological test mode best mimics the particular application and also the most appropriate parameters to use in that test. For instance, skin cream application and rubbing is a high shear rate process which is best evaluated using steady shear testing at the appropriate shear rate. Conversely to the texture in the pot, the texture is related to the underlying microstructure which is best evaluated by means of oscillatory testing or CreepCreep describes a time and temperature dependent plastic deformation under a constant force. When a constant force is applied to a rubber compound, the initial deformation obtained due to the application of the force is not fixed. The deformation will increase with time.creep testing.

A simple test to evaluate material texture under small deformations is an oscillation amplitude sweep. This can provide important information relating to sample stiffness, springiness, structural strength and deformation. Stiffness is reflected in the Complex ModulusThe complex modulus consists of two components, the storage and the loss moduli. The storage modulus (or Young’s modulus) describes the stiffness and the loss modulus describes the damping (or viscoelastic) behavior of the corresponding sample using the method of Dynamic Mechanical Analysis (DMA). complex modulus G* with higher values indicating a stiffer structure, while the phase angle δ indicates the degree of elasticity and hence springiness of the structure. This information can be presented using a simple plot of G* vs. δ as shown in Figure 1.

Diagram illustrating the relationship between complex modulus and phase angle, emphasizing material stiffness and elasticity.
1) Diagram showing simple interpretation of a G* vs. δ in terms of material properties.

Other information which can be extracted from such a test is the Yield StressYield stress is defined as the stress below which no flow occurs; literally behaves like a weak solid at rest and a liquid when yielded.yield stress and the yield StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain which relate to the structural strength and the extent of structural deformation, respectively. This information can be attained from a plot of elastic StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress σ’ (StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress associated with the Elastic (or Storage) Modulus G’) versus StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain. A peak in the elastic StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress indicates the yield point and the values of StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress and StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain measured at this point the Yield StressYield stress is defined as the stress below which no flow occurs; literally behaves like a weak solid at rest and a liquid when yielded.yield stress and yield StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain, respectively, as shown in Figure 2.

By combining all of this information, it is possible to get an indication of how a material will respond to small shear deformations before the onset of macroscopic flow.

This can be useful for benchmarking products or to help engineer specific sensory properties or functional benefits into a product.

Graph illustrating the relationship between elastic stress and strain, highlighting yield stress and yield strain points.
2) Diagram showing how an amplitude sweep can be used to determine the Yield StressYield stress is defined as the stress below which no flow occurs; literally behaves like a weak solid at rest and a liquid when yielded.yield stress and StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain

Experimental

Results and Discussion

Figure 3 compares a range of different products in terms of their relative stiffness and elasticity at a frequency of 1 Hz. From this chart, it can be seen that most samples are predominantly elastic with phase angles lower than 45º. However, these samples show varying degrees of stiffness with the body butter for example being 25 times stiffer (higher modulus) than the body lotion, and the hair gum being almost 100 times stiffer. Conversely, the shower cream is predominantly fluid-like with a phase angle close to 90º and a relatively low stiffness, with a G* value of just 23 Pa compared with approx. 8000 Pa for the body butter.

The effect of temperature on butter texture is highly significant with fat CrystallizationCrystallization is the physical process of hardening during the formation and growth of crystals. During this process, heat of crystallization is released.crystallization at low temperatures (fridge) forming a stiff and highly elastic structure while at room temperature, the melting of this fat matrix results in a softer and less elastic structure, more similar in texture to the body butter product and the toothpaste.

Table 1 shows the corresponding values of Yield StressYield stress is defined as the stress below which no flow occurs; literally behaves like a weak solid at rest and a liquid when yielded.yield stress and yield StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain for the range of products. Note that yield StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress essentially describes the StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress required to initiate breakdown of the network structure. Since viscoelastic fluids (δ > 45º) do not possess a network structure, yield StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress in this case relates to the StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress required to initiate significant flow (Shear ThinningThe most common type of non-Newtonian behavior is shear thinning or pseudoplastic flow, where the fluid vis­cosity decreases with increasing shear.shear thinning).

Table 1: Results from peak analysis of stress-strain curves

SampleYield StressYield stress is defined as the stress below which no flow occurs; literally behaves like a weak solid at rest and a liquid when yielded.Yield Stress (Pa)Yield StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.Strain (%)
Mayonnaise11.261.79
Toothpaste1.860.057
Body butter15.870.81
Body lotion2.242.63
Shower cream10.1827.22
Hair styling gum11.120.15
Butter (5°C)340001.06
Butter (25°C)1.120.096

Comparing the body butter and the body lotion, it is clear that the former requires a higher StressStress is defined as a level of force applied on a sample with a well-defined cross section. (Stress = force/area). Samples having a circular or rectangular cross section can be compressed or stretched. Elastic materials like rubber can be stretched up to 5 to 10 times their original length.stress to break down the structure. This is evident during product use, with the body butter requiring greater force to initiate flow. The body lotion has a higher yield StrainStrain describes a deformation of a material, which is loaded mechanically by an external force or stress. Rubber compounds show creep properties, if a static load is applied.strain and will deform more before thinning, suggesting a more ductile/less brittle structure. The elastic dominant mayonnaise has both a high yield stress and yield strain reflecting its observed ‘rubbery texture’ in the jar.

Although the body wash shows a high critical stress and strain, unlike the mayonnaise, it does not possess a network structure (δ > 45º). These critical values therefore relate to the stress and deformation that the material can withstand before flow is significantly enhanced. This can sometimes be related to extent of filament formation or product stringiness.

Butter at fridge temperature has a very high yield stress which is why it can be difficult to spread; however, at 25ºC a significant drop in yield stress can be observed due to melting of the crystalline fat matrix. Interestingly butter is more brittle at this higher temperature as indicated by the smaller yield strain.

Conclusion

An amplitude sweep test can provide important information relating to a materials textural property such as stiffness, springiness, structural strength and brittleness. By measuring the parameters associated with these properties it is possible to build a picture of how a material will look and behave under small deformations. Such a technique is useful for characterizing and comparing material proper.

Please note that testing is recommended to be undertaken with cone and plate or parallel plate geometry – with the latter being preferred for dispersions and emulsions with large particle sizes. Such material types may also require the use of serrated or roughened geometries to avoid artefacts relating to slippage at the geometry surface.

AI Overview
An error occurred. Please try again.