Introduction

The storage of hydrogen in cryogenic tanks requires materials that can withstand extremely low temperatures. Carbon fiber-reinforced polymer (CFRP) composites with epoxy resins as the matrix material are a promising solution for meeting the lightweight requirements of the aerospace and automotive industries. Dynamic mechanical thermal analysis (DMA) is an indispensable tool for the optimal development of these materials. This application note explains how DMA is used to evaluate and optimize epoxy resin formulations for cryogenic applications and presents the results of a recent dissertation at the Polymer Engineering Institute of the University of Bayreuth (https://www.polymer- engineering.de/) which is dedicated to this topic.

Methods and Materials

Dynamic Mechanical Thermal Analysis (DMA) was used to measure the viscoelastic properties of resin formulations over a wide temperature range down to low temperatures. The following viscoelastic parameters were recorded:

All measurements were carried out with a NETZSCH DMA Eplexor® 500 N in a temperature range from -140°C to 300°C.

Epoxy resins used: 

  • EP1: Standard epoxy resin, based on diglycidyl ether of bisphenol A (DGEBA) with polyetheramine (PEA) as hardener. This combination serves as a reference material without any additional modifications. 
  • EP2: DGEBA resin with dicyandiamide hardener (DICY) with urea accelerator. 
  • EP3: DGEBA resin with isophorondiamine (IPDA) as the cold hardener, which is also typically used in the manufacture of rotor blades. 
  • EP4: DGEBA resin with 4,4‘ diaminodiphenylsulphone (DDS) hardener for high-temperature resins in the aerospace industry. 
  • EP5: Epoxy resin, based on tetraglycidylmethylendianillin (TGMDA) with DDS hardener with higher crosslinking DensityThe mass density is defined as the ratio between mass and volume. density. 
  • EP2X: Modified version of EP2 with portions of core shell particles for modifying toughness at low temperatures.

Overview of the DMA Analysis Results

Glass Transition TemperatureThe glass transition is one of the most important properties of amorphous and semi-crystalline materials, e.g., inorganic glasses, amorphous metals, polymers, pharmaceuticals and food ingredients, etc., and describes the temperature region where the mechanical properties of the materials change from hard and brittle to more soft, deformable or rubbery.Glass Transition Temperature (Tg)

The Glass Transition TemperatureThe glass transition is one of the most important properties of amorphous and semi-crystalline materials, e.g., inorganic glasses, amorphous metals, polymers, pharmaceuticals and food ingredients, etc., and describes the temperature region where the mechanical properties of the materials change from hard and brittle to more soft, deformable or rubbery.glass transition temperature (Tg) is a critical point that defines the application limits of a material as a decrease in the storage modulus and a maximum in the Viscous modulusThe complex modulus (viscous component), loss modulus, or G’’, is the “imaginary” part of the samples the overall complex modulus. This viscous component indicates the liquid like, or out of phase, response of the sample being measurement. loss modulus or tan d. Epoxy resins with a higher degree of cross-linking have a higher Tg, which means that they retain their stiffness at higher temperatures.

Storage Modulus (E') 

The storage modulus increases with decreasing temperature (figure 1). At -196°C, the resins tested showed a significantly higher storage modulus, indicating increased stiffness. This property is important because when the modulus of the matrix changes, the behavior is expected to be significantly different from that at room temperature. This is a critical parameter in the design of tank structures.

Storage modulus E’ vs. temperature graph showing samples EP1 to EP5 with marked transition temperatures Tg, Tα, and Tβ.
1) Storage modulus E‘of all samples (EP1 to EP5) as a function of temperature from DMA Eplexor®® 500 measurements with transition temperature including Tg.

Loss Modulus (E") and Damping Factor tan δ 

The Viscous modulusThe complex modulus (viscous component), loss modulus, or G’’, is the “imaginary” part of the samples the overall complex modulus. This viscous component indicates the liquid like, or out of phase, response of the sample being measurement. loss modulus, which indicates the damping properties of the material, decreases at cryogenic temperatures. This indicates that the material dissipates less energy through internal friction at cryogenic temperatures, resulting in a more brittle characteristic. The DMA results were consistent with the fracture toughness tests at -196°C – the material becomes increasingly brittle at low temperatures and becomes increasingly linearly elastic with loss of plastic deformability (figure 2).

Loss factor tan δ graph for EP1 to EP5 showing storage modulus variations with temperature from -150°C to 200°C.
2) Loss factor tan δ as a function of temperature of EP1 to EP5.

Influence of the Toughness Modification 

The addition of toughness-modifying additives, such as nanoscale core-shell particles, improved the fracture toughness of the resins without compromising much on the required stiffness of the fiber-plastic composite at elevated temperatures. This results in a balanced combination of stiffness and toughness, which is ideal for cryogenic tanks under varying temperature loads. It can be seen that the modified resins have a lower E' value at -196°C. This means that these materials do not become as brittle and a kind of ‘residual ductility’ remains, which is important for the balance between structural integrity and increased fracture toughness of the cryogenic tanks for micro-crack resistance.

The addition of silicone nanoparticles results in softening of the network, which is indicated by a lower modulus than that of the unmodified EP2 over the entire temperature range. At low temperatures in particular, plasticization of the network can be seen via the Glass Transition TemperatureThe glass transition is one of the most important properties of amorphous and semi-crystalline materials, e.g., inorganic glasses, amorphous metals, polymers, pharmaceuticals and food ingredients, etc., and describes the temperature region where the mechanical properties of the materials change from hard and brittle to more soft, deformable or rubbery.glass transition temperature of the silicone core. The modulus is lower at all temperatures because silicone has a significantly lower stiffness than pure epoxy. The chemical compatibility between silicone and epoxy is improved by the thermoplastic shell, which causes the modulus to reduce less sharply.

The Tg is slightly reduced as softening of the network starts earlier at 5% addition (figure 3). However, after the maximum loss factor tan d, the Tg only drops to +142.9°C. The actual softening point of the material, defined by the drop in E' modulus, is +122°C. However, this is high enough for EP2X to ensure adequate safety of the composite at external temperature requirements of up to +90°C. The component stiffness up to +122°C is relevant for the assembly of bonded joints or attachments to the tank structure, as these need to be dimensionally stable at a Curing (Crosslinking Reactions)Literally translated, the term “crosslinking“ means “cross networking”. In the chemical context, it is used for reactions in which molecules are linked together by introducing covalent bonds and forming three-dimensional networks.curing temperature of, for example, +120°C, since they need to be reheated locally in order to make bonded joints for attachments or repairs.

Graph comparing loss factor tan δ for modified and unmodified resins (EP1 to EP5) across a temperature range of -200 to 300 °C.
3) Comparison of storage modulus for modified and unmodified resins.

Correlation with the Mechanical Behavior of Crogenic Tanks at -196°C

The thermo-mechanical properties determined by DMA correlate directly with the mechanical behavior of the CFRP material that can be used for cryogenic tank structures. 

The Use of DMA in Material Development for Cryogenic Tank Applications

Conclusion

Dynamic mechanical thermal analysis (DMA), or also called dynamic mechanical thermal analaysis (DMTA), is an essential tool in the development of materials for cryogenic applications. It allows detailed evaluation of the thermo-mechanical properties of epoxy resins and their optimization for use in carbon fiber-reinforced cryogenic tanks. Through systematic use of DMA, materials can be developed that can withstand the extreme requirements and offer high performance and safety. More detailed information can be found in Dr Hübner's thesis:

Modifizierte Epoxidharzformulierungen zur Herstellung von kohlenstofffaserverstärkten kryogenen Wasserstoffspeichern im automatisierten Legeverfahren - EPub Bayreuth (uni-bayreuth.de)

Literature

  1. [1]
AI Overview
An error occurred. Please try again.