30.08.2021 by Dr. Natalie Rudolph, Thomas Zenker

Thermoplastic Automated Fiber Placement (TAFP): Determination of the Degree of Crystallinity based on Position within the Process Chain

Airplane taking off on a runway, showcasing modern aviation technology. NETZSCH branding visible in the lower-left corner.

The use of continuous fiber-reinforced plastics with thermoplastic matrix systems in the aviation industry requires the development of suitable manufacturing technologies for this material combination. One promising process in this context is Automated Fiber Placement (AFP). Learn more about the process chains for the production of structural components and why the degree of Crystallinity / Degree of CrystallinityCrystallinity refers to the degree of structural order of a solid. In a crystal, the arrangement of atoms or molecules is consistent and repetitive. Many materials such as glass ceramics and some polymers can be prepared in such a way as to produce a mixture of crystalline and amorphous regions.crystallinity is decisive.

The aviation industry is constantly evolving. The use of continuous fiber-reinforced plastics with thermoplastic matrix systems requires the development of suitable manufacturing technologies for this material combination. One promising process in this context is Automated Fiber Placement (AFP), a highly automated placement process for the production of continuous fiber-reinforced composites by means of a laying head. This laying head can be mounted either on a gantry system or a robot (figure 1).

Automated Fiber Placement (AFP) plant with a gantry robot placing continuous fibers on a curved surface, showcasing advanced composite manufacturing.
Figure 1: Plant Concepts: Automated Tape Laying (ATL)/Automated Fiber Placement (AFP) (a) gantry ATL plant [1]; (b) robot-based AFP plant [2]

Thanks to the available degrees of freedom of the system, it is possible – in contrast with winding filament – to lay up on concave surfaces and follow non-geodesic fiber paths. In both cases the material can either be carried along on the head or stored in a separate, stationary enclosure (creel). In the AFP process, prepregs with both cross-linking and thermoplastic matrices can be processed.

Schematic of TAFP process chains, illustrating in-situ layup, vacuum bagging, autoclave consolidation, and thermoforming steps.
Figure 2: Process chains on a TAFP basis (a) TAFP in-situ consolidation: in-situ layup, demolding; (b) TAFP depositing in final contour with downstream consolidation: layup, vacuum bagging, consolidation in autoclave, debagging; (c) Process chain transformation of TAFP preforms: layup, clamping, preheating, thermoforming, demolding

Different Process Chains for the Production of Structural Components

For the production of structural components based on thermoplastic unidirectional tapes (UD tapes), different process chains are taken into consideration in Automated Fiber Placement. In in-situ TAFP, the objective is to achieve full consolidation of the structure during placement. The complex process control for the laying process severely limits the feasible geometry of the target components, which is why the in-situ TAFP process has so far been used primarily for simple components such as tanks, pipes or simply curved panels. More complex geometries can instead be realized by net-shape deposition with downstream consolidation in the autoclave or heating press. Alternatively, the TAFP process can also be used for depositing flat preforms, which are subsequently formed into the component’s final shape in the press-based thermoforming process and thereby consolidated. Fig. 2 shows a schematic of the described process chains.

Why the degree of crystallinity is decisive

Primarily semi-crystalline thermoplastics are used as the matrix of thermoplastic composites. A central property of these polymers is the degree of Crystallinity / Degree of CrystallinityCrystallinity refers to the degree of structural order of a solid. In a crystal, the arrangement of atoms or molecules is consistent and repetitive. Many materials such as glass ceramics and some polymers can be prepared in such a way as to produce a mixture of crystalline and amorphous regions.crystallinity, since the resulting polymer chain and crystal structure has a decisive effect on the mechanical properties of the plastic composite. Since the matrix is completely melted and re-solidified in the consolidation or forming process step, the influence of this process step on the degree of crystallinity of the component was investigated.

Automated Fiber Placement plant Coriolis C1 features an advanced robotic arm for precise composite manufacturing.
Figure 3: Automated Fiber Placement plant Coriolis C1 of Fraunhofer IGCV

How was the test specimen produced?

To this end, test specimens made of PPS/CF UD tape material from the manufacturer Celanese in Dallas, TX, USA, were deposited on the Coriolis C1 AFP machine (figure 3). The process chains TAFP deposition in final contour with downstream consolidation and Transformation of TAFP preform were sampled on a heating press by the manufacturer Langzauner (Lambrechten, Austria); additionally, specimens were consolidated in an autoclave. Table 1 summarizes the process parameters relevant for CrystallizationCrystallization is the physical process of hardening during the formation and growth of crystals. During this process, heat of crystallization is released.crystallization, i.e., pressure and cooling rate in the temperature range of the Crystallinity / Degree of CrystallinityCrystallinity refers to the degree of structural order of a solid. In a crystal, the arrangement of atoms or molecules is consistent and repetitive. Many materials such as glass ceramics and some polymers can be prepared in such a way as to produce a mixture of crystalline and amorphous regions.crystallinity band.

Table. 1: Parameters of the consolidation process (excerpt)

ProcessPressureCooling rate
Consolidation: heating press20 bar-10 K/min
Consolidation: autoclave5 bar-10 K/min
Transformation20 barUp to -2950 K/min

How was crystallinity determined?

For the determination of the Crystallinity / Degree of CrystallinityCrystallinity refers to the degree of structural order of a solid. In a crystal, the arrangement of atoms or molecules is consistent and repetitive. Many materials such as glass ceramics and some polymers can be prepared in such a way as to produce a mixture of crystalline and amorphous regions.crystallinity of the PPS matrix as a function of processing, the Differential Scanning Calorimetry method was employed. A DSC 214 Polyma by NETZSCH (Selb, Germany) was used. The samples were heated from 20°C to 320°C at a heating rate of 10 K/min. For each process chain, four samples were measured. The measurement conditions are summarized in table 2.

Table. 2: Measurement conditions  

Sample weight 15-28 mg 
Atmosphere N2 
Gas flow rate60 ml/min 
Temperature program 20°C –> 320°C (10 K/min)

Fig. 4 shows exemplary the measurement curves of the samples consolidated in the autoclave

NETZSCH Rosand RH07 is a high-performance laboratory shear mixer, ideal for precise material processing.
Figure 4: DSC measurement curves of the autoclave sample series For simpler interpretation, shifted on the abscissa

Calculation of the degree of crystallinity

The degree of Crystallinity / Degree of CrystallinityCrystallinity refers to the degree of structural order of a solid. In a crystal, the arrangement of atoms or molecules is consistent and repetitive. Many materials such as glass ceramics and some polymers can be prepared in such a way as to produce a mixture of crystalline and amorphous regions.crystallinity Xc was determined according to [3]:

Equation detailing the calculation of degree of crystallinity in thermoplastic composites. Relevant for Automated Fiber Placement research.

 

According to [4], the value of 150.4 J/g was used for the fusion enthalpy of 100% crystalline PPS.

By evaluating the first melting peak shown in figure 4, a fusion enthalpy of 18.0 J/g is obtained for sample 1. The smooth baseline before the peak means that no cold CrystallizationCrystallization is the physical process of hardening during the formation and growth of crystals. During this process, heat of crystallization is released.crystallization takes place. By means of wet chemical analysis, a fiber mass fraction of 61.32% was determined for the specimen. The Crystallinity / Degree of CrystallinityCrystallinity refers to the degree of structural order of a solid. In a crystal, the arrangement of atoms or molecules is consistent and repetitive. Many materials such as glass ceramics and some polymers can be prepared in such a way as to produce a mixture of crystalline and amorphous regions. degree of crystallinity is calculated according to formula (1):

 

Equation for calculating the degree of crystallinity (Xc) in thermoplastic composites; demonstrating an advanced manufacturing process.

 

Table 3  shows the degrees of Crystallinity / Degree of CrystallinityCrystallinity refers to the degree of structural order of a solid. In a crystal, the arrangement of atoms or molecules is consistent and repetitive. Many materials such as glass ceramics and some polymers can be prepared in such a way as to produce a mixture of crystalline and amorphous regions.crystallinity determined this way with relation to their positions within the process chain. Each of these reflects the mean value of 4 individual measurements and their standard deviation.

Table 3:          DSC Evaluation

SpecimenDegree of Crystallinity / Degree of CrystallinityCrystallinity refers to the degree of structural order of a solid. In a crystal, the arrangement of atoms or molecules is consistent and repetitive. Many materials such as glass ceramics and some polymers can be prepared in such a way as to produce a mixture of crystalline and amorphous regions.crystallinity [%]
Consolidation: heating press29.81  ± 2.02
Consolidation: autoclave29.11 ± 1.12
Transformation26.49 ± 1.65

Reduced Crystallinity of the Component from the Forming Process Chain

The degrees of Crystallinity / Degree of CrystallinityCrystallinity refers to the degree of structural order of a solid. In a crystal, the arrangement of atoms or molecules is consistent and repetitive. Many materials such as glass ceramics and some polymers can be prepared in such a way as to produce a mixture of crystalline and amorphous regions.crystallinity of the samples consolidated in the heating press and in the autoclave therefore do not differ significantly from one another. The higher consolidation pressure of the heating press thus has no effect on Crystallinity / Degree of CrystallinityCrystallinity refers to the degree of structural order of a solid. In a crystal, the arrangement of atoms or molecules is consistent and repetitive. Many materials such as glass ceramics and some polymers can be prepared in such a way as to produce a mixture of crystalline and amorphous regions.crystallinity.

In contrast, the samples manufactured in the forming process chain are less crystalline than the other samples. This can primarily be explained by the high heating rates of the process. Due to the high conductive heat loss when molten samples come into contact with the pressing tool, which is tempered at 150°C, cooling rates > 1000 K/s were measured in the region of the crystallinity band by means of thermocouples inserted in the laminate. Due to the short dwelling time of the polymer in the temperature range of CrystallizationCrystallization is the physical process of hardening during the formation and growth of crystals. During this process, heat of crystallization is released.crystallization, the chains do not have sufficient time to pack themselves closely resulting in reduced crystallinity of the component.

Thus, should differences be found in future mechanical investigations – for example, with regard to matrix-dominated characteristic values between the process chains – then crystallinity might be the reason behind them. If, however, forming is still to be selected as the process chain – for example, to achieve high production rates through short cycle times – then optimization of the process control may need to be pursued in certain cases to increase the Crystallinity / Degree of CrystallinityCrystallinity refers to the degree of structural order of a solid. In a crystal, the arrangement of atoms or molecules is consistent and repetitive. Many materials such as glass ceramics and some polymers can be prepared in such a way as to produce a mixture of crystalline and amorphous regions. degree of crystallinity.

About Fraunhofer IGCV

Fraunhofer IGCV stands for applied research with a focus on engineering, production, and multi-material solutions. We enable innovations in manufacturing processes and material sciences, machines and process chains, and factory and company networks. Our unique selling point proposition lies in interdisciplinary solutions from the fields of casting, composite, and processing technology.

References

[1]    Oldani T., “Increasing productivity in fiber placement processes,” in sae aerospace manufacturing and automated fastening conference & exhibition, North Charleston, South Carolina, USA, 2008.

[2]    Coriolis Composites, Coriolis C1 THE REFERENCE IN AUTOMATED FIBER PLACEMENT. [Online]. Available: https://www.coriolis-composites.com/fiber-placement-machines/coriolis-c1/ (accessed: Jul. 29 2019).

[3]    J. E. Spruiell, “A review of the measurement and development of crystallinity and its relation to properties in neat poly (phenylene sulfide) and its fiber reinforced composites,” 2005, doi: 10.2172/885940.

[4]    F. Sacchetti, W. J.B. Grouve, L. L. Warnet, and I. F. Villegas, “Effect of cooling rate on the interlaminar fracture toughness of unidirectional Carbon/PPS laminates,” Engineering Fracture Mechanics, 2018, doi: 10.1016/j.engfracmech.2018.02.022.