Published on 

Material Characterization of Polymers by Methods of Thermal Analysis − A Comprehensive Study on PMMI by Means of DSC, TGA and TGA-FT-IR

Introduction

Methods of thermal analysis are widely used in the field of polymers to characterize and identify materials. In this case study, PMMI was investigated by means of DSC, TGA and TGA-FT-IR. PMMI (Polymethacrylmethylimide) is a thermoplastic polymer. As it is an amorphous polymer, it features high transparency. Therefore, it can be used in specific applications such as the automotive industry for headlight modules, or more generically for optical components like light guides, lenses, fiber optics, luminaire covers, sight glasses and cover lenses.

Test Results

Compared to PMMA (Polymethylmethacrylate), PMMI has a higher heat deflection temperature, which is also reflected by the higher Glass Transition TemperatureThe glass transition is one of the most important properties of amorphous and semi-crystalline materials, e.g., inorganic glasses, amorphous metals, polymers, pharmaceuticals and food ingredients, etc., and describes the temperature region where the mechanical properties of the materials change from hard and brittle to more soft, deformable or rubbery.glass transition temperature (Tg) as compared to PMMA. Figure 1 shows the DSC results of the 2nd heating curves for PMMI in direct comparison to PMMA. For these two grades, the Tg of PMMA is at 109.1°C (midpoint) and of PMMI far higher at 175.8°C (midpoint).

DSC curve comparison of PMMA (blue) and PMMI (red) showing glass transition temperatures and specific heat changes.
1) DSC 214 Polyma results for the PMMA sample (blue curve) and for the PMMI sample (red curve) (second heating curves; heating rate: 10 K/min, sample mass: PMMA 13.98 mg, PMMI 10.64 mg). The PMMI for this study presented as an undried granulate and was investigated as received.
DSC curve analysis for PMMI showing glass transition temperatures and specific heat changes during heating at 10 K/min.
2) DSC 214 Polyma results for the PMMI sample (blue curve: first heating; red curve: second heating) (heating rate: 10 K/min, sample weight: PMMI 10.64 mg)

 

In the first heating curve of the DSC experiment (blue curve in figure 2), one can observe – besides the Glass Transition TemperatureThe glass transition is one of the most important properties of amorphous and semi-crystalline materials, e.g., inorganic glasses, amorphous metals, polymers, pharmaceuticals and food ingredients, etc., and describes the temperature region where the mechanical properties of the materials change from hard and brittle to more soft, deformable or rubbery.glass transition Tg at 162.2°C – also an EndothermicA sample transition or a reaction is endothermic if heat is needed for the conversion.endothermic effect at 197.1°C directly following the Tg. As this effect is not seen in the second heating, it can be assumed that it may be an evaporation effect of a volatile component. This can be proven in a first step just by reweighing the sample after the DSC experiment (in this case, one would find a mass loss of approx. 1%). The Glass Transition TemperatureThe glass transition is one of the most important properties of amorphous and semi-crystalline materials, e.g., inorganic glasses, amorphous metals, polymers, pharmaceuticals and food ingredients, etc., and describes the temperature region where the mechanical properties of the materials change from hard and brittle to more soft, deformable or rubbery.glass transition of the PMMI can be found in the second heating curve (red curve in figure 2) at 175.8°C (midpoint).

One thermoanalytical method for verifying the mass loss quantitatively is thermogravimetric analysis (TGA). The results for the PMMI sample are shown in figure 3. In the TGA curve, a mass-loss step of 1.0% is observed in the temperature range from RT to 260°C. The maximum of the mass-loss rate for this mass-loss step can be seen as a minimum in the DTG curve (first derivative of the TGA curve) at 199.9°C. This mass-loss step clearly corresponds to the EndothermicA sample transition or a reaction is endothermic if heat is needed for the conversion.endothermic effect that was observed at 197.1°C (peak temperature) in the first heating curve of the DSC measurement.

DSC and TGA analysis graphs for PMMI sample, showing glass transition at 162.2°C and key thermal peaks at 197.1°C and 159.9°C.
3) DSC 214 Polyma results for the PMMI sample (blue curve: first heating) and TG 209 F1 Libra® (solid black curve: TGA curve; dash-dotted black curve: DTG curve) (heating rate: 10 K/min)
TGA and DTG curves of PMMI sample show mass changes and thermal peaks at 199 °C and 190.7 °C. Analytical testing data.
4) Temperature-dependent mass change (TGA, solid black curve), rate of mass change (DTG, dash-dotted black curve) and Gram-Schmidt curve (dash-dotted red curve) of the PMMI sample

 

By means of TGA, one can quantify the mass loss at a certain temperature; it would now be of greater interest to learn what gas evolved during this mass-loss step, in order to gain deeper insight into the composition of the sample. 

To detect and identify the evolved gas, the TGA system was coupled to an FT-IR spectrometer; this can be done in a unique way with the NETZSCH PERSEUS® TG 209 F1 Libra®. The PERSEUS® coupling system is a direct coupling of the TG 209 F1 Libra® with the Bruker Alpha FT-IR spectrometer. 

Figure 4 depicts, for the coupled TGA-FT-IR measurement on PMMI, the Gram-Schmidt curve (red) along with the TGA and DTG curves. The Gram-Schmidt curve displays the overall IR intensities and behaves as a mirror image of the mass-loss rate (DTG) while also showing maximum intensities during the mass-loss steps. 

To evaluate the IR data in detail, the individual spectrum was taken at the mass-loss step at 200°C and compared to entries in the installed databases (figure 5). In this case, comparison with the library shows that the gas released is definitely H2O.

IR spectrum comparison of PMMI (blue) at 200°C and H2O library spectrum (red), highlighting key absorption peaks.
5) Extracted IR spectrum for PMMI at 200°C (blue curve) compared to library spectrum for H2O (red curve)