Published on 

Revealing Sorption/Desorption Properties of Micro-Crystalline Cellulose by Means of STA

Introduction

Moisture may affect the properties of a wide range of active ingredients and excipients in terms of their stability, Crystallinity / Degree of CrystallinityCrystallinity refers to the degree of structural order of a solid. In a crystal, the arrangement of atoms or molecules is consistent and repetitive. Many materials such as glass ceramics and some polymers can be prepared in such a way as to produce a mixture of crystalline and amorphous regions.crystallinity, bio-availability, etc. One method for determining the influence of humidity on a substance’s behavior is dynamic vapor Sorption ProcessSorption is a physical and chemical process by which a substance (typically a gas or liquid) accumulates within another phase or on the phase boundary of two phases. Depending on the place of accumulation, a differentiation is made between absorption (accumulation in a phase) and adsorption (accumulation at the phase boundary).sorption (DVS), in which the mass changes in the sample are measured for different solvent vapor amounts, e.g., water vapor. [1] 

Such measurements can be carried out with an STA (simultaneous thermal analyzer) connected to a modular humidity generator (figure 1). In the following, a dynamic water Sorption ProcessSorption is a physical and chemical process by which a substance (typically a gas or liquid) accumulates within another phase or on the phase boundary of two phases. Depending on the place of accumulation, a differentiation is made between absorption (accumulation in a phase) and adsorption (accumulation at the phase boundary).sorption measurement was carried out on micro-crystalline cellulose (MCC, chemical structure in figure 2). This substance is used in tablet formulations as filler and binder. [2]

Netsch STA 449 Nevio thermal analysis instrument with digital display, showcasing precise measurement capabilities for material testing.
Modular humidity generator (MHG) with digital display for precise humidity control and temperature measurement.
1) STA 449 F3 Nevio and modular humidity generator
Square sample holder with a wooden top, featuring a metal base and a knob for secure fastening, on a concrete surface.
2) Chemical structure of micro-crystalline cellulose

Measurement Conditions

The experimenal conditions are summarized in table 1.


Table 1: Conditions of the test

Device

STA 449 F3 Nevio connected with the humidity generator

Sample

Micro-crystalline cellulose

Sample mass

41.22 mg

Sample holder

Plate made of alumina, Ø 17 mm

Temperature program

IsothermalTests at controlled and constant temperature are called isothermal.Isothermal 44°C, nitrogen atmosphere, relative humidity (RH) increased

from 0 to 80%

Measurement Results

Figure 3 displays the measured sample mass and temperature during the experiment. 

The results demonstrate the strong hygroscopic nature of the micro-crystalline cellulose. The first increase in relative humidity from 0% to 20% (blue dashed curve) induces a mass increase of 4% (green curve). The subsequent steps show that the higher the relative humidity, the higher the mass gain. As soon as the humidity level decreases, the absorbed and/or adsorbed water is released, resulting in a mass loss. When a completely dry atmosphere is finally reached at the end of the measurement, the amount of water absorbed and/or adsorbed will have been quantitatively released. This can be confirmed by having arrived back at the initial sample mass (100%). 

Each change in relative humidity level is associated with a peak in the sample temperature curve (pink curve). This is due to the ExothermicA sample transition or a reaction is exothermic if heat is generated.exothermal and endothermal natures of the Sorption ProcessSorption is a physical and chemical process by which a substance (typically a gas or liquid) accumulates within another phase or on the phase boundary of two phases. Depending on the place of accumulation, a differentiation is made between absorption (accumulation in a phase) and adsorption (accumulation at the phase boundary).sorption and desorption of water, respectively.

Mass and temperature data graph for micro-crystalline cellulose under varying humidity levels (0%-80%).
3) Mass and temperature results for micro-crystalline cellulose in an atmosphere with different humidity levels (0%, 20%, 40%, 60% and 80%)

The mass gain and loss after reaching equilibrium are given in figure 4 for all measured relative humidity levels between 0% and 80%. The maximum mass increase amounts to 12% for a relative humidity of 80%. Microcrystalline cellulose exhibits Sorption ProcessSorption is a physical and chemical process by which a substance (typically a gas or liquid) accumulates within another phase or on the phase boundary of two phases. Depending on the place of accumulation, a differentiation is made between absorption (accumulation in a phase) and adsorption (accumulation at the phase boundary).sorption hysteresis, i.e., the water amount in the sample is higher during desorption than during Sorption ProcessSorption is a physical and chemical process by which a substance (typically a gas or liquid) accumulates within another phase or on the phase boundary of two phases. Depending on the place of accumulation, a differentiation is made between absorption (accumulation in a phase) and adsorption (accumulation at the phase boundary).sorption (see figure 4) but, ultimately, the starting point and ending point of the Sorption ProcessSorption is a physical and chemical process by which a substance (typically a gas or liquid) accumulates within another phase or on the phase boundary of two phases. Depending on the place of accumulation, a differentiation is made between absorption (accumulation in a phase) and adsorption (accumulation at the phase boundary).sorption/desorption cycle are identical.

This hysteresis phenomenon is typical for many porous materials. Chen et al [3] showed that the water-cellulose bonds formed during swelling of cellulose do not break upon desorption at the same chemical potential.

DSC graph displaying the crystallization behavior of PBT at varying cooling rates, highlighting temperature peaks and transitions.
4) Difference in the moisture content of the sample between Sorption ProcessSorption is a physical and chemical process by which a substance (typically a gas or liquid) accumulates within another phase or on the phase boundary of two phases. Depending on the place of accumulation, a differentiation is made between absorption (accumulation in a phase) and adsorption (accumulation at the phase boundary).sorption and desorption