| Veröffentlicht: 

One Measurement, Two Signals: cp Determination and Curie Detection on Iron with the STA 509 Jupiter®

Introduction

Pure iron is frequently used as a reference and test material in materials science. Its well-known thermophysical and metallurgical properties make it suitable for validating measurement methods and for investigating correlations between microstructure, magnetism and thermal behavior.

In addition to temperature-dependent specific heat capacity, cp, the ferromagnetic-paramagnetic transition at the Curie temperature is of particular interest. This transformation affects the thermophysical behavior of iron and appears as a characteristic effect in the heat-capacity curve.

The STA 509 Jupiter® simultaneously acquires thermal and gravimetric signals by DSC-TGA. Combined with a magnetic setup, it enables precise cp determination and clear detection of the Curie transformation of pure iron from the TGA signal within a single measurement.

Close view of the STA furnace equipped with the magnetic setup used for Curie detection.
STA furnace with magnetic setup

Experiment and Measurement Conditions

The measurements were performed on an iron sample with the STA 509 Jupiter® under argon. Specific heat capacity was determined by DSC cp evaluation while the TGA signal was recorded in parallel. A magnetic setup was used to detect the Curie transformation.

Table 1: STA measurement parameters

ParameterCondition
InstrumentSTA 509 Jupiter®
Measuring headType S TGA/DSC
FurnaceRhodium
CruciblePt/Rh crucible with lid and Al2O3 liner
AtmosphereAr with OTS®, 70 ml/min
Temperature program
Sample mass121.871 mg
Calibration standardSapphire, 55.203 mg

Evaluation of Specific Heat Capacity

Specific heat capacity, cp, is determined by a comparative method using a reference material, as described, for example, in DIN EN ISO 11357. The evaluation requires three separate measurements: a baseline, a standard material and the sample.

Reproducible baseline and sapphire measurements are essential because they form the basis for the subsequent calculation. From these data sets, the temperature-dependent cp value of the investigated material is obtained. The result provides a basis for material characterization and can be used as an input parameter for further thermophysical calculations.

cp=signal difference(sample−baseline)sample mass·heating rate·sensitivity

At the same time, the measurement is conducted with the magnetic setup. The combination of TGA and DSC signals provides a particularly clear and well-supported detection of the magnetic transformation.

Temperature-dependent cp curve of pure iron in blue, literature cp values in red and TGA curve in green showing the Curie transition and the alpha-iron to gamma-iron transformation.
Temperature-dependent cp curve (blue), literature cp values [1] (red), TGA curve (green).

Results and Discussion

The measured specific heat capacity of pure iron initially shows the expected continuous increase. Up to approximately 700°C, the experimental values agree very well with literature data. This confirms the quality of the cp determination and the suitability of the STA 509 Jupiter® for thermophysical measurements on metallic materials.

In the range of the Curie transformation, the cp curve exhibits a characteristic effect that is assigned to the ferromagnetic-paramagnetic transition of iron. The peak temperature is approximately 771°C. A further transformation effect, the solid-state transformation α-Fe → γ-Fe, is visible at 918°C. This second-order phase transition produces a pronounced change in the heat-capacity curve and permits determination of the transformation temperature.

Independent Curie Detection by TGA

The TGA curve was recorded simultaneously with the cp measurement using a magnetic setup. In the ferromagnetic state, pure iron interacts with the applied magnetic field. At the Curie temperature, iron changes to the paramagnetic state and the magnetically induced force acting on the sample changes abruptly. The TGA curve consequently shows an apparent mass increase.

This signal is not caused by a real mass change. Below the Curie temperature, the sample is attracted by the magnet. Above the Curie temperature, iron loses its ferromagnetic properties; the additional force no longer acts on the sample and is registered as a change in the TGA signal.

The temperature of the characteristic TGA signal correlates very well with the Curie transformation in the cp curve. The magnetic setup therefore provides independent confirmation of the magnetic phase transition. Without a magnetic field, no relevant mass change is expected in the investigated temperature range because the sample is measured in a gas-tight system under inert atmosphere, excluding OxidationOxidation kann im Zusammenhang mit thermischer Analyse verschiedene Vorgänge bezeichnen.oxidation-related or other mass-changing processes.

Key Measurement Results

The concurrent cp and TGA signals support confident interpretation of magnetic and structural transformations in pure iron.

Literature agreement
Measured cp data agree very well with literature values up to approximately 700°C.
Curie transformation
The ferromagnetic-paramagnetic transition is detected at approximately 771°C in the cp and TGA signals.
Solid-state transformation
The α-Fe → γ-Fe transformation is visible as a pronounced cp effect at 918°C.

Conclusion

The investigation of iron demonstrates that the STA 509 Jupiter® can determine specific heat capacity reliably and accurately. The measured cp values agree very well with literature data. In addition, the Curie transformation is detected simultaneously in the cp curve and, with the magnetic setup, in the TGA curve.

The characteristic increase in the TGA signal at the Curie temperature correlates closely with the transformation effect in the heat-capacity curve. This agreement makes the magnetic transformation visible on two independent signal levels and strengthens confidence in the interpretation.

For material characterization, an appropriate measurement setup enables thermal and magnetically induced effects to be investigated in one experiment. This is particularly relevant for iron-based materials and the analysis of magnetic transformations.

References

[1] NETZSCH-Gerätebau GmbH: NETZSCH Proteus® software, “Spezifische Wärmekapazität (cp)Die spezifische Wärmekapazität oder Wärmekapazität ist eine messbare physikalische Größe, die dem Verhältnis der einem Objekt zugeführten Wärme zur resultierenden Temperaturänderung entspricht.cp Standard – Pure Iron”, reference data stored in 2006, accessed through Proteus® on June 11, 2026, version 9.9.0, Selb, Germany.

Related Devices

Explore the STA 509 Jupiter® instrument family for simultaneous DSC and TGA measurements in material characterization.

  • STA 509 Jupiter® Classic

    Bestes Preis/Leistungs-Verhältnis

    • RT bis 1600 °C
    • SiC-Ofen
    • Auflösung der Waage: 0,1 μg
    • Optionaler ASC mit 20 Positionen
  • STA 509 Jupiter® Select

    Auf individuelle Bedürfnisse zugeschnitten

    • -150 °C bis 2400 °C
    • Auswahl aus 12 verschiedenen Öfen
    • Auflösung der Waage: 0,1 μg
    • Optionaler ASC mit 20 Positionen oder zweiter Ofen
  • STA 509 Jupiter® Supreme

    Instrument für Höchstleistungen

    • -150 °C bis 2000 °C
    • Auswahl aus 9 verschiedenen Öfen
    • Auflösung der Waage: 0,025 μg
    • Optionaler ASC mit 20 Positionen oder zweiter Ofen
  • STA 319 Jupiter®

    Zugang zur simultanen thermischen Analyse

    • RT (10°C) bis 1025°C/1100°C an der Probe
    • Robuster schnell heizender und kühlender Ofen
    • Waagenauflösung: 20 ng
    • Optionaler 204-Position ASC

Download

Download Application Note 457 for the complete measurement description, measurement parameters, cp and TGA curves, and reference information.

    AI Overview
    An error occurred. Please try again.