Published on 

Detecting Weak Thermal Effects by Means of Differential Scanning Calorimetry

Introduction

Differential scanning calorimetry (DSC) is a popular method to characterize thermal effects as melting, CrystallizationCrystallization is the physical process of hardening during the formation and growth of crystals. During this process, heat of crystallization is released.crystallization or Glass Transition TemperatureThe glass transition is one of the most important properties of amorphous and semi-crystalline materials, e.g., inorganic glasses, amorphous metals, polymers, pharmaceuticals and food ingredients, etc., and describes the temperature region where the mechanical properties of the materials change from hard and brittle to more soft, deformable or rubbery.glass transition and many more. 

The DSC signal is proportional to the Specific Heat Capacity (cp)Heat capacity is a material-specific physical quantity, determined by the amount of heat supplied to specimen, divided by the resulting temperature increase. The specific heat capacity is related to a unit mass of the specimen.specific heat capacity of the material being measured, and also to the heating rate and the sample mass. The Specific Heat Capacity (cp)Heat capacity is a material-specific physical quantity, determined by the amount of heat supplied to specimen, divided by the resulting temperature increase. The specific heat capacity is related to a unit mass of the specimen.specific heat capacity is a material size and can therefore not be changed. The Glass Transition TemperatureThe glass transition is one of the most important properties of amorphous and semi-crystalline materials, e.g., inorganic glasses, amorphous metals, polymers, pharmaceuticals and food ingredients, etc., and describes the temperature region where the mechanical properties of the materials change from hard and brittle to more soft, deformable or rubbery.glass transition is a change in Specific Heat Capacity (cp)Heat capacity is a material-specific physical quantity, determined by the amount of heat supplied to specimen, divided by the resulting temperature increase. The specific heat capacity is related to a unit mass of the specimen.specific heat capacity and can typically be detected as a small effect in the DSC curve. A possibility to magnify this or other small effects is to increase the sample mass. If the amount of material available is limited, using a sensitive DSC – a stable baseline proveided – allows for detecting small effects even with only a small sample quantity.

Table 1: Measurement conditions

Device

DSC 300 Caliris® with H-Module

Sample mass10.38 mg1.07 mg131 μg80 μg
Crucible

Concavus® (aluminum, closed with pierced lid)

Temperature range

25°C to 180°C

Heating rate

10 K/min

Atmosphere

Nitrogen (20 ml/min)

Measurement Results

Figure 1 depicts the DSC resulting curve of the 10.38-mg sample. The Glass Transition TemperatureThe glass transition is one of the most important properties of amorphous and semi-crystalline materials, e.g., inorganic glasses, amorphous metals, polymers, pharmaceuticals and food ingredients, etc., and describes the temperature region where the mechanical properties of the materials change from hard and brittle to more soft, deformable or rubbery.glass transition is detected as an endothermal step at 87.1°C (midpoint). It is related to a change in Specific Heat Capacity (cp)Heat capacity is a material-specific physical quantity, determined by the amount of heat supplied to specimen, divided by the resulting temperature increase. The specific heat capacity is related to a unit mass of the specimen.specific heat capacity of 0.3 J/(g·K).

DSC curve analysis showing glass transition of 10.38 mg PS at 87.1°C with specific heat change indicated.
1) DSC curve during heating. The step-line change in the DSC curve represents the Glass Transition TemperatureThe glass transition is one of the most important properties of amorphous and semi-crystalline materials, e.g., inorganic glasses, amorphous metals, polymers, pharmaceuticals and food ingredients, etc., and describes the temperature region where the mechanical properties of the materials change from hard and brittle to more soft, deformable or rubbery.glass transition of the polymer.

Figure 2 compares the previous measurement (blue curve) to the tests performed on lower masses. The lower the sample mass, the smaller the glass transition appears. However, it results, of course, in the same Specific Heat Capacity (cp)Heat capacity is a material-specific physical quantity, determined by the amount of heat supplied to specimen, divided by the resulting temperature increase. The specific heat capacity is related to a unit mass of the specimen.specific heat capacity change because this one is not depending on the mass.

DSC graph showing glass transition analysis of polystyrene at different sample masses, highlighting temperature and heat flow.
2) Determination of the glass transition of polystyrene for different sample masses

Summary

The sensitive sensor of the DSC 300 Caliris® allows for detection of small effects even for small sample masses. Due to the larger sample mass, the glass transition effect in the DSC curve can be better recognized higher. This improves evaluation and precision of the Glass Transition TemperatureThe glass transition is one of the most important properties of amorphous and semi-crystalline materials, e.g., inorganic glasses, amorphous metals, polymers, pharmaceuticals and food ingredients, etc., and describes the temperature region where the mechanical properties of the materials change from hard and brittle to more soft, deformable or rubbery.glass transition temperature.